Jump to content

Specific Process Knowledge/Characterization/XRD/XRD Powder: Difference between revisions

From LabAdviser
Reet (talk | contribs)
Process information: ny underside
Eves (talk | contribs)
 
(12 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/XRD/XRD_Powder click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/XRD/XRD_Powder click here]'''
<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b><br>
All images and photos on this page belongs to <b>DTU Nanolab</b></i>


=The XRD Powder setup=
=The XRD Powder setup=
[[Image:machine front with on-off button.JPG|right|thumb|300px|The XRD Powder located in the basement of building 346 at Nanolab, Room 904.]]
[[Image:machine front with on-off button.JPG|right|thumb|300px|The XRD Powder located in the basement of building 346 at Nanolab, Room 904.]]
The "XRD powder" is an Aeris Research edition benchtop X-ray diffractometer from Malvern Panalytical. It is meant for phase analysis of powders, is easy to use, and offers the option of making measurements while heating the sample in a N<sub><sub>2</sub></sub> atmosphere. The setup allows X-ray diffraction measurements in Bragg-Brentano mode (i.e., Theta-2Theta measurements where the incident and diffraction arms of the goniometer are coupled). We have a very limited selection of optics for this instrument, so there is little that the user can adjust.
The "XRD powder" is an Aeris Research edition benchtop X-ray diffractometer from Malvern Panalytical. It is meant for phase analysis of powders and is easy to use. The setup allows X-ray diffraction measurements with a Cu source in Bragg-Brentano mode (i.e., Theta-2Theta measurements where the incident and diffraction arms of the goniometer are coupled). We have a very limited selection of optics for this instrument, so there is little that the user can adjust.
 
Special capabilities:
 
* The instrument has a 1D strip detector, which makes data acquisition quicker.
* It is possible to load up to 6 samples at a time and program the measurements so the machine loads and measures them automatically one after another.
* The detector has a fluorescence suppression option for measuring samples with iron and other substances that fluoresce under copper radiation.
* Sample heating up to 500° C possible in N<sub>2</sub>.
* Transmission measurements possible.


Please contact the equipment responsible if you would like to mount the special sample holder for heating during the measurement.  
Please contact the equipment responsible if you would like to mount the special sample holders for heating or transmission measurements.  


'''The user manual(s), user APV(s), technical information, and contact information can be found in LabManager:'''  
'''The user manual(s), user APV(s), technical information, and contact information can be found in LabManager:'''  


[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=463 XRD Powder in LabManager]
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=463 XRD Powder in LabManager] - requires login




==Process information==
==Process information==


*Tips for choosing among the scan and hardware parameters you are allowed to change: [[/Measurement tips| XRD Powder meausurement tips]]
*Tips for choosing among the scan and hardware parameters including fluorescence suppression: [[/Measurement tips| XRD Powder measurement tips]]


*Malvern Panalytical has a large collection of webinars on XRD. You have to register to view them but the amount of email you receive afterwards is modest, so it's worth it in my opinion (Rebecca, July 2022). Some useful webinars include:
*Malvern Panalytical has a large collection of webinars on XRD. You have to register to view them but the amount of email you receive afterwards is modest, so it's worth it in my opinion (Rebecca, July 2022). Some useful webinars include:
Line 31: Line 42:
|-
|-
!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"| Crystal structure analysis and thin film thickness measurement
|style="background:LightGrey; color:black"| Crystal structure analysis
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Phase ID
*Phase ID
Line 68: Line 79:
0.4 mm x 12 mm (Line)
0.4 mm x 12 mm (Line)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="5"|Goniometer
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Goniometer
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|
Scanning mode
Scanning mode
Line 89: Line 100:
Fixed with rotation
Fixed with rotation
|-
|-
|style="background:LightGrey; color:black"|
 
Sample size
|style="background:WhiteSmoke; color:black"|
Powders
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Optics
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Optics
|style="background:LightGrey; color:black"|Incident side
|style="background:LightGrey; color:black"|Incident side
Line 123: Line 130:


<br clear="all" />
<br clear="all" />
==Anton Paar Heating Stage BTS - 500==
If required, the ambient stage can be replaced with a heating cell unit, enabling powder samples to be heated up to 500 °C under vacuum or in an inert atmosphere. The gas-flow chemistry can also be modified using a dedicated bubbler connected to the gas lines.
[[/Anton Paar BTS-500| Anton Paar BTS-500 heating stage]]

Latest revision as of 14:32, 18 June 2026

Feedback to this page: click here

Unless otherwise stated, this page is written by DTU Nanolab internal
All images and photos on this page belongs to DTU Nanolab

The XRD Powder setup

The XRD Powder located in the basement of building 346 at Nanolab, Room 904.

The "XRD powder" is an Aeris Research edition benchtop X-ray diffractometer from Malvern Panalytical. It is meant for phase analysis of powders and is easy to use. The setup allows X-ray diffraction measurements with a Cu source in Bragg-Brentano mode (i.e., Theta-2Theta measurements where the incident and diffraction arms of the goniometer are coupled). We have a very limited selection of optics for this instrument, so there is little that the user can adjust.

Special capabilities:

  • The instrument has a 1D strip detector, which makes data acquisition quicker.
  • It is possible to load up to 6 samples at a time and program the measurements so the machine loads and measures them automatically one after another.
  • The detector has a fluorescence suppression option for measuring samples with iron and other substances that fluoresce under copper radiation.
  • Sample heating up to 500° C possible in N2.
  • Transmission measurements possible.

Please contact the equipment responsible if you would like to mount the special sample holders for heating or transmission measurements.

The user manual(s), user APV(s), technical information, and contact information can be found in LabManager:

XRD Powder in LabManager - requires login


Process information

  • Malvern Panalytical has a large collection of webinars on XRD. You have to register to view them but the amount of email you receive afterwards is modest, so it's worth it in my opinion (Rebecca, July 2022). Some useful webinars include:

Software

To adjust measurement parameters and analyze the data, you will need dedicated software which is described here: XRD Powder software

Equipment performance and process related parameters

Equipment XRD Powder
Purpose Crystal structure analysis
  • Phase ID
  • Crystal Size
  • Crystallinity
X-ray generator

Maximum rated output

600 W

Rated tube voltage

40 kV

Rated tube current

15 mA

Type

Sealed tube

Target

Cu

Focus size

0.4 mm x 12 mm (Line)

Goniometer

Scanning mode

incident / receiver coupled

Goniomenter radius

145 mm

Minimum step size

0.001° (3.6")

Sample stage

Fixed with rotation

Optics Incident side
  • 0.04° soller slit
  • Ni and Cu filter
  • Divergence slits
  • Beam mask
Receiver side
  • 0.04° soller slit
  • Ni filter
Substrates Measurement temperature

May be heated in N2 up to 500 °C

Substrate size

Only for powders

Allowed materials

All materials have to be approved



Anton Paar Heating Stage BTS - 500

If required, the ambient stage can be replaced with a heating cell unit, enabling powder samples to be heated up to 500 °C under vacuum or in an inert atmosphere. The gas-flow chemistry can also be modified using a dedicated bubbler connected to the gas lines.


Anton Paar BTS-500 heating stage