AZ MiR 701 is a positive UV photoresist.
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/MiR click here]'''
 
[[Category: Lithography|Resist]]
[[Category: Resist|AZ MiR 701]]
 
__TOC__
 
==Resist description==
AZ MiR 701 is a positive UV photoresist. It is considered to have high selectivity for dry etching.


==Spin coating==
==Spin coating==
[[Image:MiRspincurves.JPG|640px|thumb|Spin curves for AZ MiR 701 (29 cps) using a 30 s spin-off, and a 60 s @ 90°C proximity softbake]]


[[Image:MiRspincurves.JPG|500x500px|thumb|Spin curves for AZ MiR 701 (29cps) using a 30s spin-off, and a 60s@90°C softbake (proximity bake for Gamma)]]
'''Typical spin parameters:'''
*Spin off: 30-60 s
*Soft bake: 60 s @ 90°C in proximity
<br clear="all" />


<br clear="all" />
==Exposure==
'''Dehydration of resist film:'''<br>
During exposure in the maskless aligners, MiR can be sensitive to dehydration by the air flow applied by the pneumatic auto-focus mechanism. This may lead to insufficient development, especially for small substrates. This problem can be alleviated by switching to the overview camera for a period of 1 minute before starting the exposure, or simply by parking the writehead away from the exposure location for 1 minute before starting the exposure. Dehydration can also mess up a dose test, but this can be fixed by increasing the spacing between the individual doses, or even better by extending the test design to 40mm or more in the Y-direction (adding a very small structure in the design file, or increasing the upper boarder during conversion).
 
The effect can also be reduced by increasing the soft bake.


==Post-exposure bake==
==Post-exposure bake==
'''Typical PEB parameters:'''
*PEB temperature: 110°C
*PEB time: 60 s
During exposure, interaction between the incoming light and the light reflected by the substrate can cause a standing wave to form in the resist (especially true for single line/wavelength exposure). This leads to a wavy sidewall after development. The standing wave pattern can be reduced by introducing a post-exposure bake before development, which allows the activated PAC to diffuse into un-activated regions, thus smoothing the sidewall. The recommended PEB for MiR is 60 s at 110°C (for a 1 - 2 µm film). Thicker coatings may require longer bake, and substrate thickness and material may also affect the required baking time.


During exposure, interaction between the incoming light and the light reflected by the substrate can cause a standing wave to form in the resist (especially true for single line/wavelength exposure). This leads to a wavy sidewall after development. The standing wave pattern can be removed by introducing a post-exposure bake before development, which allows the activated PAC to diffuse into un-activated regions, thus smoothing the sidewall. The recommended PEB for MiR is 60s at 110°C.
Since the post-exposure bake is at an elevated temperature compared to the soft bake, it will cause the resist film to become 5-10% thinner (probably due to continued evaporation of solvent). A 1.5 µm thick MiR resist film will be approximately 1.4 µm after PEB.


As the post-exposure bake is at an elevated temperature compared to the soft bake, it will cause the resist film to become 5-10% thinner (probably due to continued evaporation of solvent). A 1.5µm thick MiR resist film will be approximately 1.4µm after PEB.
<gallery style="text-align: center;" widths=450 heights=350>
MIR_noPEB.jpg|1.5 µm AZ MIR 701 without PEB
MIR_withPEB.jpg|1.5 µm AZ MIR 701 with PEB
</gallery>


==Development==
==Development==
 
'''Development speed:'''
A 1.5-2µm MiR resist film is fully developed in 60s using TMAH (AZ 726). Thicker coatings will require longer development (1 min per 2µm).
*Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min

Latest revision as of 14:39, 5 May 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Resist description

AZ MiR 701 is a positive UV photoresist. It is considered to have high selectivity for dry etching.

Spin coating

Spin curves for AZ MiR 701 (29 cps) using a 30 s spin-off, and a 60 s @ 90°C proximity softbake

Typical spin parameters:

  • Spin off: 30-60 s
  • Soft bake: 60 s @ 90°C in proximity


Exposure

Dehydration of resist film:
During exposure in the maskless aligners, MiR can be sensitive to dehydration by the air flow applied by the pneumatic auto-focus mechanism. This may lead to insufficient development, especially for small substrates. This problem can be alleviated by switching to the overview camera for a period of 1 minute before starting the exposure, or simply by parking the writehead away from the exposure location for 1 minute before starting the exposure. Dehydration can also mess up a dose test, but this can be fixed by increasing the spacing between the individual doses, or even better by extending the test design to 40mm or more in the Y-direction (adding a very small structure in the design file, or increasing the upper boarder during conversion).

The effect can also be reduced by increasing the soft bake.

Post-exposure bake

Typical PEB parameters:

  • PEB temperature: 110°C
  • PEB time: 60 s


During exposure, interaction between the incoming light and the light reflected by the substrate can cause a standing wave to form in the resist (especially true for single line/wavelength exposure). This leads to a wavy sidewall after development. The standing wave pattern can be reduced by introducing a post-exposure bake before development, which allows the activated PAC to diffuse into un-activated regions, thus smoothing the sidewall. The recommended PEB for MiR is 60 s at 110°C (for a 1 - 2 µm film). Thicker coatings may require longer bake, and substrate thickness and material may also affect the required baking time.

Since the post-exposure bake is at an elevated temperature compared to the soft bake, it will cause the resist film to become 5-10% thinner (probably due to continued evaporation of solvent). A 1.5 µm thick MiR resist film will be approximately 1.4 µm after PEB.

Development

Development speed: