Jump to content

Specific Process Knowledge/Lithography/Development/manualTMAH developer: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Jehem (talk | contribs)
 
(12 intermediate revisions by the same user not shown)
Line 1: Line 1:
{{cc-nanolab}}
=Developer: TMAH Manual 02=
=Developer: TMAH Manual 02=
[[file:Developer_TMAH_manual_02.jpg|400px|right|thumb|Developer: TMAH Manual 02 is located in E-4.]]
[[file:Developer_TMAH_manual_02.jpg|400px|right|thumb|Developer: TMAH Manual 02 is located in E-4.]]
Line 4: Line 6:
'''Tool description'''<br>
'''Tool description'''<br>
The Developer: TMAH manual 02 is a semi-automatic and programmable single substrate developer system, which can be used for development of resists on chips, 50 mm, 100 mm and 150 mm substrates. The development is done using AZ 726 MIF, which is a 2.38% TMAH solution with wetting agent.
The Developer: TMAH manual 02 is a semi-automatic and programmable single substrate developer system, which can be used for development of resists on chips, 50 mm, 100 mm and 150 mm substrates. The development is done using AZ 726 MIF, which is a 2.38% TMAH solution with wetting agent.
Single substrates are loaded manually into the tool, but the developer dispense, puddle time, agitation, rinse and drying is controlled by the tool.


{| class="wikitable"
{| class="wikitable"
! style="text-align:left" | Product:
! style="text-align:left" | Product
| style="padding-left: 10px" | Laurell EDC-650-HZB-23NP
| style="padding-left: 10px" | Laurell EDC-650-HZB-23NP
|-
|-
! style="text-align:left" | Year of purchase:   
! style="text-align:left" | Year of purchase  
| style="padding-left: 10px" | 2016
| style="padding-left: 10px" | 2016
|-
|-
! style="text-align:left" | Tool modification:
! style="text-align:left" | Tool modification
| style="padding-left: 10px" | Modified from e-beam solvent developer to UV TMAH developer in 2024
| style="padding-left: 10px" |  
Converted from e-beam solvent developer to UV TMAH developer in 2024<br>
Added media flow controllers for developer, rinse and drying media in 2025
|-
|-
! style="text-align:left" | Location:
! style="text-align:left" | Location
| style="padding-left: 10px" | Cleanroom E-4
| style="padding-left: 10px" | Cleanroom E-4
|}
|}


'''User manual'''<br>
'''User manual'''<br>
The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager] - '''requires login'''
The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=341 LabManager] - '''requires login'''


'''Tool training'''<br>
'''Tool training'''<br>
Training on the tool requires users to complete the [https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Lithography#Lithography_Tool_Package_Training lithography TPT] followed by the online tool training and a hands-on authorization training.  
Training on the tool requires users to complete the [https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Lithography#Lithography_Tool_Package_Training lithography TPT] followed by the online tool training and a hands-on authorization training.<br>
 
The tool training video is part of the online tool training, but can also be viewed [https://www.youtube.com/watch?v=btinNzYnLnY here].
The tool training video is part of the online tool training, but can also be viewed [https://www.youtube.com/watch?v=btinNzYnLnY here].
<br clear="all" />
<br clear="all" />
Line 76: Line 81:
! scope=row style="text-align: left;" | Substrate batch size
! scope=row style="text-align: left;" | Substrate batch size
| 1
| 1
|-
! scope=row style="text-align: left;" | Media flow rates
|
*AZ 726 MIF (TMAH): 300 ml/min
*Process DI water: 400 ml/min
*Backside rinse DI water: 140 ml/min
*Process Nitrogen: 20 l/min
|}
|}
<br clear="all" />
<br clear="all" />


=Process information=
=Process information=
All recipes use the following structure:
All recipes use the following structure:
#Pressurize the TMAH canister
#Pressurize the TMAH canister
#Pre-wet substrate at high RPM
#Dispense puddle while rotating substrate slowly
#Dispense puddle while rotating substrate slowly
#Puddle development with agitation of substrate
#Puddle development with agitation of substrate
Line 90: Line 102:




Multipuddle recipes repeat steps 2-4 for the given number of puddles.
'''Multi puddle'''<br>
 
Multi puddle recipes repeat steps 2-4 for the given number of puddles.


==Process recipes==
==Process recipes==
Line 147: Line 159:
| colspan="2"|AZ 726 MIF (2.38% TMAH)
| colspan="2"|AZ 726 MIF (2.38% TMAH)
|}
|}
<br clear="all" />
<br clear="all"/>

Latest revision as of 08:47, 11 March 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Developer: TMAH Manual 02

Developer: TMAH Manual 02 is located in E-4.

Tool description
The Developer: TMAH manual 02 is a semi-automatic and programmable single substrate developer system, which can be used for development of resists on chips, 50 mm, 100 mm and 150 mm substrates. The development is done using AZ 726 MIF, which is a 2.38% TMAH solution with wetting agent.

Single substrates are loaded manually into the tool, but the developer dispense, puddle time, agitation, rinse and drying is controlled by the tool.

Product Laurell EDC-650-HZB-23NP
Year of purchase 2016
Tool modification

Converted from e-beam solvent developer to UV TMAH developer in 2024
Added media flow controllers for developer, rinse and drying media in 2025

Location Cleanroom E-4

User manual
The user manual and contact information can be found in LabManager - requires login

Tool training
Training on the tool requires users to complete the lithography TPT followed by the online tool training and a hands-on authorization training.
The tool training video is part of the online tool training, but can also be viewed here.

Equipment performance and process related parameters

Tool purpose

Development of UV resists:

  • AZ nLOF 2020
  • AZ MIR 701
  • AZ 5214E
  • AZ 4562

Development of DUV resists:

  • KrF M230Y
  • KrF M35G
Developer AZ 726 MIF (2.38% TMAH)
Development method Puddle
Handling method
  • Non-vacuum chuck for 100 mm & 150 mm wafers
  • Non-vacuum chuck for chips and 50 mm wafers
Process temperature Room temperature
Process agitaion 15 cycles per minute
Process rinse DI water
Substrate sizes
  • Chips
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Substrate materials
  • All cleanroom allowed materials
  • Film, or pattern, of all materials except Type IV
Substrate batch size 1
Media flow rates
  • AZ 726 MIF (TMAH): 300 ml/min
  • Process DI water: 400 ml/min
  • Backside rinse DI water: 140 ml/min
  • Process Nitrogen: 20 l/min


Process information

All recipes use the following structure:

  1. Pressurize the TMAH canister
  2. Pre-wet substrate at high RPM
  3. Dispense puddle while rotating substrate slowly
  4. Puddle development with agitation of substrate
  5. Spin off developer
  6. Clean substrate and chamber with DI water
  7. Dry substrate and chamber with nitrogen


Multi puddle
Multi puddle recipes repeat steps 2-4 for the given number of puddles.

Process recipes

(Updated 2026-01-12, JEHEM)

  • -Rinse-
  • 1x015s
  • 1x030s
  • 1x060s
  • 1x120s
  • 2x060s
  • 5x060s

Agitation

Testing showed that adding agitation to the puddle step gave better uniformity in the development rate over the entire area of the substrate as well as increased development rate.

Tests were performed on under-exposed resist, specifically for showing the difference between the agitation and non-agitation puddle development - the measured results cannot necessarily be transferred directly to a working process, only the vague general behavior of the two process setups; faster/slower development speed and better/worse uniformity across substrate.

Development rate for under-exposed resist test
Non-uniformity for under-exposed resist test
Non-agitation Agitation
Test results
  • Slower development
  • Worse uniformity
  • Faster development
  • Better uniformity
Normalized development rate 1 1.20
Non-uniformity 21% 11%
Agitation None 15 cycles per minute, 20 rpm, 500 rpm/s
Substrate 100 mm SSP silicon
Resist film 1.5 µm AZ 5214E
Exposure dose 50 mJ/cm2 (~50% of normal dose)
Development Single puddle for 60 seconds
Developer AZ 726 MIF (2.38% TMAH)