'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Gold click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Gold click here]''' | ||
Gold can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the different deposition equipment. We also describe the temperature rise on the wafer during gold deposition, the adhesion layers that can be used for gold deposition, the roughness of gold deposited in the Wordentec, and issues with particulates on the gold films in the Temescal and the Wordentec. | Gold can be deposited by e-beam evaporation or sputtering. In the chart below you can compare the different deposition equipment. We also describe the temperature rise on the wafer during gold deposition, the adhesion layers that can be used for gold deposition, the roughness of gold deposited in the Wordentec, and issues with particulates on the gold films in the Temescal and the Wordentec. | ||
| Line 13: | Line 13: | ||
! | ! | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]]) | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]]) | ||
! Resistive thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal Evaporator]]) | ! Resistive thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal Evaporator]]) | ||
! Sputter ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ! Sputter ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]]) | ||
| Line 21: | Line 20: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! General description | ! General description | ||
| E-beam deposition of Au | | E-beam deposition of Au | ||
| Resistive thermal deposition of Au | | Resistive thermal deposition of Au | ||
| Line 34: | Line 32: | ||
| | | | ||
| | | | ||
|RF Ar clean | |RF Ar clean | ||
| | | | ||
| Line 40: | Line 37: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Layer thickness | ! Layer thickness | ||
|10 Å to | |10 Å to 600 nm * | ||
|10 Å to 200 nm | |10 Å to 200 nm | ||
|10 Å to | |10 Å to 500 nm * | ||
|10 Å to | |10 Å to 500 nm * | ||
| very thin, few nm range | | very thin, few nm range | ||
| very thin, few nm range | | very thin, few nm range | ||
| Line 51: | Line 47: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Deposition rate | ! Deposition rate | ||
| | |1-5 Å/s | ||
|1 Å/s (can be adjusted to around 5 Å/s) | |||
|1 Å/s (can be adjusted to around | |||
|Depends on process parameters, 1-10 Å/s | |Depends on process parameters, 1-10 Å/s | ||
|Depends on process parameters | |Depends on process parameters | ||
| Line 67: | Line 62: | ||
*Up to 3x8" wafers (ask for special holder) | *Up to 3x8" wafers (ask for special holder) | ||
*many smaller pieces | *many smaller pieces | ||
| | | | ||
*4x2" wafers or | *4x2" wafers or | ||
| Line 94: | Line 85: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Heating | |||
|to 250 C (in 10-pocket evaporator) | |||
|no | |||
|no | |||
|to 600 C | |||
|no | |||
|no | |||
|-style="background:WhiteSmoke; color:black" | |||
!Allowed materials | !Allowed materials | ||
| | | | ||
*See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet] | *See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet] | ||
| | | | ||
* Almost any as long as it does not outgas - see cross-contamination sheets in Labmanager | * Almost any as long as it does not outgas - see cross-contamination sheets in Labmanager | ||
| Line 127: | Line 119: | ||
* All samples allowed in the SEM Supra 2 or 3 | * All samples allowed in the SEM Supra 2 or 3 | ||
|-style="background: | |-style="background:LightGrey; color:black" | ||
! Comment | ! Comment | ||
| | | | ||
* | * Pumpdown approx 20 min. | ||
| | | | ||
*Make sure that all pellets are melted beforehand | *Make sure that all pellets are melted beforehand | ||
*Pumpdown approx. 20 min | |||
| | | | ||
*Takes approx. 10 minutes to load and transfer sample | *Takes approx. 10 minutes to load and transfer sample | ||
| Line 150: | Line 140: | ||
''' | '''*''' ''For thicknesses above 200 nm write to metal@nanolab.dtu.dk as extra deposition costs a higher fee.'' | ||
== Resistive thermal evaporation of Au == | == Resistive thermal evaporation of Au == | ||
| Line 191: | Line 149: | ||
The adhesion of gold on Silicon or Silicon with native oxide is not very good. The Si substrate is often deposited an adhesion layer before the gold deposition. A few nm of Chromium or Titanium works well and they react with the Oxygen of Silicon oxide and present a metallic bond with gold. You can also use polymer or organosilane adhesion layers as exemplified by the work in the next section. | The adhesion of gold on Silicon or Silicon with native oxide is not very good. The Si substrate is often deposited an adhesion layer before the gold deposition. A few nm of Chromium or Titanium works well and they react with the Oxygen of Silicon oxide and present a metallic bond with gold. You can also use polymer or organosilane adhesion layers as exemplified by the work in the next section. | ||
For Cr and Ti adhesion layers, a 5 nm to 10 nm thick layer | For Cr and Ti adhesion layers, a 5 nm to 10 nm thick layer is commonly used and it is important to deposit Cr or Ti and then immediately Au. If the vacuum chamber is opened in between, the surface of Cr or Ti will get oxidized and that will give a poor adhesion. If a gold layer needs to be deposited directly on Silicon, then native oxide has to be removed by a dip in diluted HF and wafer must be immediately loaded into the evaporation chamber. And after the deposition, the wafer has to be heated up to get some Au-Si diffusion which improves the adhesion. | ||
*[[/Adhesion layers|Read more about Ti and Cr adhesion layers]]. | *[[/Adhesion layers|Read more about Ti and Cr adhesion layers]]. | ||
== Thin Au layer using APTMS adhesion layer and sputter system Lesker == | == Thin Au layer using APTMS adhesion layer and sputter system Lesker == | ||
| Line 262: | Line 218: | ||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | {| border="1" cellspacing="2" cellpadding="2" colspan="3" | ||
|bgcolor="#98FB98" |'''Quality control (QC) for the Temescal''' | |bgcolor="#98FB98" |'''Quality control (QC) for the E-beam Evaporator (Temescal) and the E-beam Evaporator (10-pockets)''' | ||
|- | |- | ||
| | | | ||
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=429 QC procedure | TiAu or CrAu is tested approximately once a month on both of Nanolab's e-beam evaporators. | ||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=429 | |||
'''You can find the QC procedures and data in LabManager here''' (requires login): | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=429 QC procedure, E-beam Evaporator (Temescal)]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=429 Newest QC data, E-beam Evaporator (Temescal)]<br> | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5862&mach=511 QC procedure, E-beam Evaporator (10-pockets)]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=511 Newest QC data, E-beam Evaporator (10-pockets)]<br> | |||
{| {{table}} | {| {{table}} | ||
| align=" | | align="left" valign="top"| | ||
{| border=" | {| border="2" cellspacing="1" cellpadding="2" align="left" style="width:400px" | ||
! QC Recipe: | ! QC Recipe: | ||
! Standard recipes/TiAu or Cr/Au | ! Standard recipes/TiAu or Cr/Au | ||
|- | |- | ||
|Deposition rate | |Deposition rate | ||
| | |2 Å/s | ||
|- | |- | ||
|Thickness | |Thickness | ||
| Line 285: | Line 249: | ||
|- | |- | ||
|} | |} | ||
| align=" | |- | ||
{| border="2" cellspacing="1" cellpadding="2" align=" | |} | ||
{| {{table}} | |||
| align="left" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="left" style="width:400px" | |||
!QC limits | !QC limits | ||
! | !Both e-beam evaporators | ||
|- | |- | ||
|Deposition rate deviation | |Deposition rate deviation | ||
| Line 302: | Line 271: | ||
|- | |- | ||
|} | |} | ||
Thickness is measured in 5 points with a stylus profiler. <br> | Thickness is measured in 5 points with a stylus profiler. <br> | ||
Additionally we examine the newly deposited films for particles using the particle scanner (if available, otherwise we use the Jenatech microscope in darkfield mode) and we monitor the sheet resistance of the Ti/Au or Cr/Au films. | Additionally we examine the newly deposited films for particles using the particle scanner (if available, otherwise we use the Jenatech microscope in darkfield mode) and we monitor the sheet resistance of the Ti/Au or Cr/Au films. | ||
|} | |} | ||