Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus: Difference between revisions

Jmli (talk | contribs)
Jmli (talk | contribs)
No edit summary
 
(201 intermediate revisions by 4 users not shown)
Line 1: Line 1:
'''Feedback to this page:  
'''Feedback to this page:  
[mailto:plasma@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus click here]'''
[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus click here]'''
[[Category: Equipment |Etch DRIE]]
[[Category: Equipment |Etch DRIE]]
[[Category: Etch (Dry) Equipment|DRIE]]
[[Category: Etch (Dry) Equipment|DRIE]]


= The DRIE Pegasus tools at DTU Nanolab =
{{Template:Author-jmli1}}
<!--Checked for updates on 2/02-2023 - ok/jmli -->
<!--Checked for updates on 21/10-2025 - ok/jmli -->


== The DRIE Pegasus at Danchip ==
In 2010 DTU Nanolab acquired DRIE-Pegasus 1. As a state-of-the-art etch tool with excellent performance and great flexibility, it grew immensely popular and by 2015 it was apparent that we needed yet another tool to cope with the demand. Therefore, in 2016 Pegasus 2 was acquired from a closed-down lab and installed next to Pegasus 1.


[[Image:DRIE-Pegasus.jpg |300x300px|thumb|The SPTS Pegasus in the Danchip cleanroom A-1]]
Looking to expand our dry etching capabilities in 2017 we got an irresistible offer on a twin Pegasus system with cassette to cassette vacuum robot from a commercial fab. The twin Pegasus system (called Pegasus 3 and 4) is installed at the old cluster 2 location in cleanroom C1 and will run only 6" wafers. Pegasus 3 is the 6" silicon etch work horse and Pegasus 4 is converted (adding extra process gases) into a 6" dielectric etch tool that will supplement/replace the AOE.


'''The Bosch process'''
This page was originally intended as a regular one-machine page (the Pegasus 1 page). However, as of 2018 with several tools, the page will serve as common page for all of our Pegasi with subpages for each tool.


The DRIE Pegasus is a state-of-art silicon dry etcher that offers outstanding performance in terms of etch rate, uniformity etc. It uses the so-called Bosch process to achieve excellent control of the etched features. Click [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description|HERE]] for more fundamental information of the system.
{|
 
|width="100"| [[file:DRIE-Pegasus.jpg |100px|frameless]]
=== Change of showerhead in December 2014 ===
| width="200"| [[file:Pegasus 2 operator.jpg |204px|frameless]]
 
| width="275"|[[file:Peg3and4 front 2.JPG |292px|frameless]]
 
|-  
The showerhead that distributes the process gasses inside the plasma source has been changed. With the new design the gas flow resistance in the gas line from MFC to plasma has been reduced. This has very little or no impact on processes that have a continuous gas flow - i.e. processes that are not switched. However, for processes with several gas flows that switch on and off, the switching from one gas flow to another will be much more well defined. This enables us to run Bosch processes with shorter cycles times. Shorter cycles times means smaller scallops and hence lower roughness and better control.
| align="center" | The DRIE-Pegasus 1 load lock and cassette loader in the DTU Nanolab cleanroom A-1. {{photo1}}
 
| align="center" | The DRIE-Pegasus 2 operator station and load lock in the DTU Nanolab cleanroom A-1. {{photo1}}
As stated, we believe that only switched processes will be affected by this change. Continuous processes such as [[Specific Process Knowledge/Etch/DRIE-Pegasus/processC|Process C]], [[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano142|Nano1.42]], isotropic etches, barc etches or the black silicon recipes are not believed to be noticeably affected.
| align="center" | The DRIE-Pegasus3 and DRIE-Pegasus4 operator station and cassette loading stations. {{photo1}}
 
|-
Click [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange|HERE]] to see a comparison of some the etches before and after the change of the showerhead.
|}
 
 
'''The user manual(s), quality control procedure(s) and results, user APV(s), technical information and contact information can be found in LabManager:'''
 
Equipment info in [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=265| LabManager]
 
== Process information ==
 
'''Process notation'''
 
Describing a process recipe on the Pegasus may sometimes be difficult because of the great flexibility of the instrument. A compact and precise notation is therefore required for the recipes. Click [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Notation|here]] to find a short description of the official SPTS notation.
 
'''[[Specific Process Knowledge/Etch/DRIE-Pegasus/StandardRecipes|Standard recipes]]'''
 
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/processA|Process A (Large trench): 80 µm wide trench etched down to a depth of 150 µm]]
 
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/processB|Process B (Via etch): 30 µm diameter via etched down to a depth of 100 µm]]
 
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/processC|Process C (Nano etch): 50-300 nm posts]]
 
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/processD|Process D (Micro stamp) ''Please note that this process has changed'' ]]
 
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/SOIetch|SOI etch]]
 
'''Hardware changes'''
 
A few hardware modifications have been made on the Pegasus since it was installed in 2010. The changes are listed below.
 
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange|Change of showerhead in December 2014]]
 
'''Other etch processes'''
 
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch|Nanoetch]]
 
More processes, such as for DUV resist, are currently being developed, but they are not quite 'ready for publication' at LabAdviser so please contact Jonas (mailto:jml@danchip.dtu.dk) for more information.
 
<!--  *[[Specific Process Knowledge/Etch/DRIE-Pegasus/slopedsidewalls|Etches that produce positively sloped sidewalls for imprinting purposes]] -->
 
<!-- *[[Specific Process Knowledge/Etch/DRIE-Pegasus/Waferthinning| Maskless reduction of wafer thicknesses]] -->
 
<!-- *[[Specific Process Knowledge/Etch/DRIE-Pegasus/VeeryDeeep| Very deep etching]] -->
 
'''Advanced Processing - Henri Jansen style'''
*[[/Advanced Processing|Details on Advanced processing - Henri Jansen style Click here]]
 
'''Wafer bonding'''
 
To find information on how to bond wafers or chips to a carrier wafer, click [[Specific Process Knowledge/Etch/DryEtchProcessing/Bonding| here]].
 
'''Acceptance test'''
 
The instrument was opened for users in April 2010 when the acceptance test was signed. This was based on the performance of five standard recipes (A, B, C, D and SOI) that are further examined below. The acceptance test report is found [[Media:Pegasus_AcceptanceTest.pdf|here]].
 
'''Characterisation of etched trenches'''
 
Comparing differences in etched trenches requires a set of common parameters for each trench. Click [[Specific Process Knowledge/Etch/DRIE-Pegasus/TrenchCharacterisation|here]] to find more information about the parameters used on the DRIE-Pegasus process development.
 
'''Material from SPTS'''


*[[Specific Process Knowledge/Etch/DRIE-Pegasus/SPTSdocs|Hardware and process applications]]
== The Bosch process ==


*[[Specific Process Knowledge/Etch/DRIE-Pegasus/FAQ|Miscellaneous information]]
The DRIE Pegasus tools are state-of-art silicon dry etchers that offer outstanding performance in terms of etch rate, uniformity etc. They use the so-called Bosch process to achieve excellent control of the etched features. Click [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description|'''HERE''']] to access the top of the page. The contents are:
# [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#Description_of_the_Bosch_process_at_the_DRIE-Pegasus| Description of the Bosch process ]]
# [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#Processing_options_on_the_Pegasus | Processing options on the Pegasus ]]
# [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#Modification_of_the_showerhead | Modification of the showerhead ]]
# [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#RF_Matching | RF matching ]]
## [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#RF_matching_in_general | RF matching in general ]]
## [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/System-description#Why_RF_matching_is_extremely_important_in_the_Bosch_process | Why RF matching is extremely important in the Bosch process ]]
# [[Specific Process Knowledge/Etch/DRIE-Pegasus/picoscope|Picoscope process monitoring]]
As of 2017, completing the [[LabAdviser/Courses/TPT_Dry_Etch| Dry Etch TPT course]] is mandatory for all new users. On the TPT web page you will find a version of the latest lecture slides - here you will find information as well.


'''Internal Danchip Process log'''
== Links to the individual pages for the Pegasi ==


Process log at Danchip [http://labintra.danchip.dtu.dk/index.php/Main_Page/Process_Logs/jmli/Pegasus]
* [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-1|DRIE-Pegasus 1]]
* [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-2|DRIE-Pegasus 2]]
* [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-3|DRIE-Pegasus 3]]
* [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Pegasus-4|DRIE-Pegasus 4]]


==Equipment performance and process related parameters==
==Equipment performance and process related parameters==


{| border="2" cellspacing="0" cellpadding="2"  
{| border="2" cellspacing="0" cellpadding="1"  


!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
|style="background:WhiteSmoke; color:black"|<b>DRIE-Pegasus</b>
|style="background:silver; color:black" width="250" align ="center" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-1| '''DRIE-Pegasus 1''']]
|style="background:silver; color:black" width="250" align ="center" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-2| '''DRIE-Pegasus 2''']]
|style="background:silver; color:black" width="250" align ="center" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-3| '''DRIE-Pegasus 3''']]
|style="background:silver; color:black" width="250" align ="center" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4| '''DRIE-Pegasus 4''']]
|-
|-
!style="background:silver; color:black;" align="center" width="80"|Purpose  
!style="background:silver; color:black;" align="center" valign="center" width="100" rowspan="2"|Purpose  
|style="background:LightGrey; color:black"| Dry etch of
|style="background:Whitesmoke; color:black" width="80" | Primary
|style="background:WhiteSmoke; color:black"|  
|style="background:WhiteSmoke; color:black"|  
* Silicon
* Dry etching of 4" silicon
* Barc
* Dry etching of barc
|style="background:WhiteSmoke; color:black"|
* Research tool
|style="background:WhiteSmoke; color:black"|
* Dry etching of 6" silicon
|style="background:WhiteSmoke; color:black"|
* Dry etching of 6" dielectrics
|-
|style="background:LightGrey; color:black"|Alternative
|style="background:LightGrey; color:black"|
* Black silicon
|style="background:LightGrey; color:black"|
* Backup dry etching of 6" silicon
|style="background:LightGrey; color:black"|
* ?
|style="background:LightGrey; color:black"|
* silicon
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance
|style="background:LightGrey; color:black"|Etch rates
|style="background:whitesmoke; color:black"|Etch rates
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* Standard processes A and B up to 15 µm/min depending on etch load and feature size
* Standard processes A and B up to 15 µm/min depending on etch load and feature size
* Other processes: Any number from 200 nm/min to 10 µm/min
* Other processes: Any number from 200 nm/min to 10 µm/min
|style="background:WhiteSmoke; color:black"|
* ?
|style="background:WhiteSmoke; color:black"|
* ?
|style="background:WhiteSmoke; color:black"|
* Depending on the recipe
|-
|-
|style="background:LightGrey; color:black"|Uniformity
|style="background:LightGrey; color:black"|Uniformity
|style="background:WhiteSmoke; color:black"|
|style="background:lightgrey; color:black"|
* For standard processes better than 3 % across a 150 mm wafer.
* For standard processes better than 3 % across a 150 mm wafer.
|style="background:lightgrey; color:black"|
* ?
|style="background:lightgrey; color:black"|
* ?
|style="background:lightgrey; color:black"|
* Depending on the recipe
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Process parameter range
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Process parameter range
|style="background:LightGrey; color:black"|RF powers
|style="background:whitesmoke; color:black"|RF powers
|style="background:WhiteSmoke; color:black"|
* Coil Power 5 kW
* Platen power 300/500 W (HF/LF)
|style="background:WhiteSmoke; color:black"|
* Coil Power 5 kW
* Platen power 300/500 W (HF/LF)
|style="background:WhiteSmoke; color:black"|
* Coil Power 5 kW
* Platen power 300/500 W (HF/LF)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* Coil Power 5 kW
* Coil Power 5 kW
Line 118: Line 115:
|-
|-
|style="background:LightGrey; color:black"|Gas flows
|style="background:LightGrey; color:black"|Gas flows
|style="background:WhiteSmoke; color:black"|
|style="background:lightgrey; color:black"|
* SF<sub>6</sub>: 0 to 1200 sccm
* SF<sub>6</sub>: 0 to 1200 sccm
* O<sub>2</sub>: 0 to 200 sccm
* O<sub>2</sub>: 0 to 200 sccm
* C<sub>4</sub>F<sub>8</sub>: 0 to 400 sccm
* C<sub>4</sub>F<sub>8</sub>: 0 to 400 sccm
* Ar: 0 to 283 sccm
* Ar: 0 to 283 sccm
|style="background:lightgrey; color:black"|
* SF<sub>6</sub>-1: 0 to 1200 sccm
* SF<sub>6</sub>-2: 0 to 100 sccm
* O<sub>2</sub>: 0 to 50 sccm
* N<sub>2</sub>: 0 to 500 sccm
* Ar: 0 to 283 sccm
* He: 0 to 11 sccm
|style="background:lightgrey; color:black"|
* SF<sub>6</sub>-1: 0 to 1200 sccm
* SF<sub>6</sub>-2: 0 to 100 sccm
* O<sub>2</sub>: 0 to 200 sccm
* C<sub>4</sub>F<sub>8</sub>: 0 to 400 sccm
* Ar: 0 to 283 sccm
|style="background:lightgrey; color:black"|
{|
*SF<sub>6</sub>: ?(<20) sccm
*O<sub>2</sub>: 200 sccm
*C<sub>4</sub>F<sub>8</sub>: 400 sccm
*Ar: 283 sccm
*He: 500 sccm
*CF<sub>4</sub>: 100 sccm
*H2: 100 sccm
|
|
|}
|-
|-
|style="background:LightGrey; color:black"|Pressure and temperature
|style="background:whitesmoke; color:black"|Pressure and temperature
|style="background:WhiteSmoke; color:black"|
* Pressure range 4 to 250 mTorr
* Temperature range -20 to 30 degrees C
|style="background:WhiteSmoke; color:black"|
* Pressure range 4 to 250 mTorr
* Temperature range -20 to 30 degrees C
|style="background:WhiteSmoke; color:black"|
* Pressure range 4 to 250 mTorr
* Temperature range -20 to 30 degrees C
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* Pressure range 4 to 250 mTorr
* Pressure range 4 to 250 mTorr
Line 130: Line 161:
|-
|-
|style="background:LightGrey; color:black"|Process options
|style="background:LightGrey; color:black"|Process options
|style="background:WhiteSmoke; color:black"|
|style="background:lightgrey; color:black"|
* Bosch processes with etch and dep cycles possibly split into three individually controllable parts
* Bosch processes with etch and dep cycles each split into three
* Parameter ramping during process steps
* SOI option to reduce notching at buried oxide layers
* Picoscope monitoring
* Claritas endpoint detection system
|style="background:lightgrey; color:black"|
* Bosch processes with etch and dep cycles each split into three
* Parameter ramping during process steps
* SOI option to reduce notching at buried oxide layers
* Picoscope monitoring
* Verity OES
|style="background:lightgrey; color:black"|
* Bosch processes with etch and dep cycles each split into three
* Parameter ramping during process steps
* Picoscope monitoring
* SOI option to reduce notching at buried oxide layers
|style="background:lightgrey; color:black"|
* Bosch processes with etch and dep cycles each split into three
* Parameter ramping during process steps
* Parameter ramping during process steps
* SOI option to reduce notching at buried
* Verity OES
|-
|-
 
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:whitesmoke; color:black"|Sizes
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
* Smaller than 100mm: Bonded to carriers
* 100 mm wafers: Up to 25 wafers in a batch process
|style="background:WhiteSmoke; color:black"|
* Smaller than 150mm: Bonded to carriers
* 150 mm wafers
|style="background:WhiteSmoke; color:black"|
* Smaller than 150mm: Bonded to carriers
* 150 mm wafers
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*<nowiki>#</nowiki> small samples on carriers
* Smaller than 150mm: Bonded to carriers
*<nowiki>#</nowiki> 50 mm wafers: Bonded to carriers
* 150 mm wafers
*<nowiki>#</nowiki> 100 mm wafers: Up to 18 wafers in a batch process
|-
*<nowiki>#</nowiki> 150 mm wafers: 1 wafer
| style="background:Lightgrey; color:black"|Loading
|style="background:lightgrey; color:black"|
* Load lock
* MACS (Multiplex Atmospheric Cassette System)
|style="background:lightgrey; color:black"|
* Load lock
|style="background:lightgrey; color:black" colspan="2"|
* Vacuum cassette loader with two cassette stations and shared dealer chamber with Brooks robot
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
| style="background:Whitesmoke; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
|style="background:Whitesmoke; color:black"|
* Silicon wafers
* Quartz wafers need a (semi)conducting layer for clamping
|style="background:Whitesmoke; color:black"|
* Silicon wafers
* Quartz wafers need a (semi)conducting layer for clamping
|style="background:Whitesmoke; color:black"|
* Silicon wafers
* Quartz wafers need a (semi)conducting layer for clamping
|style="background:Whitesmoke; color:black"|
* Silicon wafers
* Silicon wafers
* Quartz wafers need a (semi)conducting layer for clamping
* Quartz wafers need a (semi)conducting layer for clamping
|-
|-
| style="background:LightGrey; color:black"|Possible masking materials
| style="background:LightGrey; color:black"|Possible masking materials
|style="background:WhiteSmoke; color:black"|
|style="background:LightGrey; color:black"|
* AZ photoresist
* zep resist
* DUV stepper resist (barc + krf)
* Oxides and nitrides
* Aluminium (only very gentle processes such as process C and nanoetches)
|style="background:LightGrey; color:black"|
* AZ photoresist
* AZ photoresist
* zep resist
* zep resist
* DUV stepper resist (barc + krf)
* DUV stepper resist (barc + krf)
* Oxides and nitrides
* Oxides and nitrides
* Aluminium (only very mild processes such as process C and nanoetches)
* Aluminium (only very gentle processes)
|style="background:LightGrey; color:black"|
* AZ and MiR photoresist
* zep resist
* DUV stepper resist (barc + krf)
* Oxides and nitrides
|style="background:LightGrey; color:black"|
* AZ photoresist
* zep resist
* DUV stepper resist (barc + krf)
* Silicon,Oxides and nitrides
* Al, Cr masks
|-
|}
|}
== Process information ==
===Process notation===
Describing a process recipe on the Pegasus may sometimes be difficult because of the great flexibility of the instrument. A compact and precise notation is therefore required for the recipes. Click [[Specific_Process_Knowledge/Etch/DRIE-Pegasus/Notation|'''HERE''']] to find a short description.
===Hardware changes===
A few hardware modifications have been made on the Pegasus 1 since it was installed in 2010. The changes are listed in the table below under hardware options.
{| border="2" cellspacing="1" cellpadding="1" align="center"
! style="background:silver; color:black" |
! style="background:silver; color:black" | [[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-1| DRIE-Pegasus 1]]
! style="background:silver; color:black" | [[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-2| DRIE-Pegasus 2]]
! style="background:silver; color:black" | [[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-3| DRIE-Pegasus 3]]
! style="background:silver; color:black" | [[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4| DRIE-Pegasus 4]]
|- valign="top"
! style="background:lightgrey; color:black" | Manufactured
| style="background:lightgrey; color:black" | 2010
| style="background:lightgrey; color:black" | 2010
| style="background:lightgrey; color:black" | 2010
| style="background:lightgrey; color:black" | 2010
|- valign="top"
! style="background:Whitesmoke; color:black" | Serial
| style="background:WhiteSmoke; color:black" | MP0636
| style="background:WhiteSmoke; color:black"| MP0641
| style="background:WhiteSmoke; color:black"| CP0170
| style="background:WhiteSmoke; color:black"| CP0171
|- valign="top"
! style="background:lightgrey; color:black" | Electrode size
| style="background:lightgrey; color:black" | 4"
| style="background:lightgrey; color:black" | 6"
| style="background:lightgrey; color:black" | 6"
| style="background:lightgrey; color:black" | 6"
|- valign="top"
! style="background:Whitesmoke; color:black" | Hardware options
| style="background:WhiteSmoke; color:black" |
* [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange|High flow plenum]]
* [[Specific Process Knowledge/Etch/DRIE-Pegasus/picoscope|Picoscope oscilloscope]]
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/Claritas|Claritas optical endpoint system]]
| style="background:WhiteSmoke; color:black"|
* [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange|High flow plenum]]
* [[Specific Process Knowledge/Etch/DRIE-Pegasus/picoscope|Picoscope oscilloscope]]
| style="background:WhiteSmoke; color:black"|
* [[Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange|High flow plenum]]
* [[Specific Process Knowledge/Etch/DRIE-Pegasus/picoscope|Picoscope oscilloscope]]
| style="background:WhiteSmoke; color:black"| ?
|-
|}
= General Pegasus information =
==Wafer bonding==
To find information on how to bond wafers or chips to a carrier wafer, click [[Specific Process Knowledge/Etch/DryEtchProcessing/Bonding| '''HERE''']].
==Characterisation of etched trenches==
The trenches in deep silicon trenches can be characterized in many ways. Being able to compare processes requires that a set of common measurements and calculations must be established. Click '''HERE''' to find more information about the parameters used on the DRIE-Pegasus process developme[[Specific Process Knowledge/Etch/DRIE-Pegasus/TrenchCharacterisation|nt]].