Specific Process Knowledge/Characterization/Optical characterization: Difference between revisions
| (74 intermediate revisions by 4 users not shown) | |||
| Line 1: | Line 1: | ||
{{cc-nanolab}} | |||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/Optical_characterization click here]''' | |||
[[Category: Equipment |Characterization Optical]] | |||
[[Category: Characterization|Optical]] | |||
==Comparison of the methods== | |||
For comparison of the methods for measuring optical constants and film thickness, see here: [[Specific Process Knowledge/Characterization/Measurement of film thickness and optical constants#Film_thickness_and_optical_constants_of_optical_transparent_films|Film thickness and optical constants of optical transparent films]] | |||
==Ellipsometer VASE and Ellipsometer M-2000V == | ==Ellipsometer RC2, Ellipsometer M2000XI (VASE) and Ellipsometer M-2000V == | ||
[[image:Ellipsometer_VASE_image.JPG|275x275px|right|thumb|Ellipsometer VASE: positioned in cleanroom | ''This section is written by Berit Herstrøm @ DTU Nanolab'' | ||
[[image:RC2 system.jpg|275x275px|right|thumb|Ellipsometer RC2: positioned in cleanroom A-1, {{photo1}}]] | |||
[[image:Ellipsometer_VASE_image.JPG|275x275px|right|thumb|Ellipsometer VASE: positioned in cleanroom C-1, {{photo1}}]] | |||
The ellipsometer VASE is a | The ellipsometer RC2 from J.A. Woollam Co., Inc is the newest of our ellipsometers. It performs slightly better then the M2000 and can measure the full Müller matrix. For most users the differences are very small. The ellipsometer VASE is actually a M2000XI-210 ellipsometer from J.A. Woollam Co., Inc.. We call it VASE (Variable Angle Spectroscopic Ellipsometry) because it can do spectroscopic ellipsometry at variable angles. <br/> | ||
The ellipsometer M2000V is an in-situ ellipsometer from J.A. Wollam Co., Inc. | The ellipsometer M2000V is an in-situ ellipsometer from J.A. Wollam Co., Inc. This dedicated for being used on the Sputter System Lesker instrument or the ALD2 for in-situ measurements. When it is not on any system it is positioned next to the ALD2. | ||
Ellipsometry is a very sensitive characterization technique which can be used to determine thin film layer thicknesses and/or optical constants. It sends in polarized light on the surface at different angles and measures the change in polarization state of the reflected light. | Ellipsometry is a very sensitive characterization technique which can be used to determine thin film layer thicknesses and/or optical constants. It sends in polarized light on the surface at different angles and measures the change in polarization state of the reflected light. | ||
| Line 14: | Line 21: | ||
Ellipsometry is an indirect measurement so a model has to be fit to the data in order to obtain the film thickness and optical constants. To learn more about ellipsometry you can take a look at the [http://www.jawoollam.com/tutorial_1.html tutorial] provided by the J. A. Woollam Co. | Ellipsometry is an indirect measurement so a model has to be fit to the data in order to obtain the film thickness and optical constants. To learn more about ellipsometry you can take a look at the [http://www.jawoollam.com/tutorial_1.html tutorial] provided by the J. A. Woollam Co. | ||
Access to use the CompleteEASE software can be found using Remote Desktop connection to: DTU-8CC0321MFL (you can only log on when you have the user competences in LabManager) or log on to https://remote.dtu.dk. There should be a connection via Citrix to DTU-8CC0321MFL. You will be prompted for user/password. | |||
| Line 20: | Line 30: | ||
<!-- give the link to the equipment info page in LabManager: --> | <!-- give the link to the equipment info page in LabManager: --> | ||
[http://labmanager. | [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=542 LabManager page for Ellipsometer RC2] <br/> | ||
[http://labmanager | [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=316 LabManager page for Ellipsometer VASE] <br/> | ||
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=261 LabManager page for Ellipsometer M-2000V] | |||
<br clear="all" /> | <br clear="all" /> | ||
===More details=== | |||
* Before training: | |||
** First go through the Woollam short tutorial: [http://www.jawoollam.com/tutorial_1.html tutorial] | |||
** Second watch our training video: [https://www.youtube.com/watch?v=EC-oyRhKr0A Training Video] | |||
** To get more understanding - short intro from ''Quantum Design - Europe'': [https://qd-europe.com/dk/en/product/short-introduction-ellipsometry/] - ''optional'' | |||
*[[/advanced ellipsometry|Examples of advanced use of the ellipsometer]] | |||
===A rough overview of the performance of the Ellipsometers=== | ===A rough overview of the performance of the Ellipsometers=== | ||
| Line 30: | Line 47: | ||
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment | !colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment | ||
|style="background:WhiteSmoke; color:black"|<b>Ellipsometer VASE</b> | |style="background:WhiteSmoke; color:black"|<b>Ellipsometer RC2</b> | ||
|style="background:WhiteSmoke; color:black"|<b>Ellipsometer VASE (M2000XI)</b> | |||
|style="background:WhiteSmoke; color:black"|<b>Ellipsometer M-2000V</b> | |style="background:WhiteSmoke; color:black"|<b>Ellipsometer M-2000V</b> | ||
|- | |- | ||
!style="background:silver; color:black;" align="center" width="60"|Purpose | !style="background:silver; color:black;" align="center" width="60"|Purpose | ||
|style="background:LightGrey; color:black"| | |style="background:LightGrey; color:black"| | ||
|style="background:WhiteSmoke; color:black"| | |||
*Measure thinfilm thicknesses and optical constants for single and multilayer optical transparent thinfilms. | |||
*Measure opticals constants for bulk material. | |||
*Measure thinfilm thicknesses and optical constants at elevated temperature <300C | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Measure thinfilm thicknesses and optical constants for single and multilayer optical transparent thinfilms. | *Measure thinfilm thicknesses and optical constants for single and multilayer optical transparent thinfilms. | ||
| Line 44: | Line 66: | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance | !style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance | ||
|style="background:LightGrey; color:black"|Films that can be examined | |style="background:LightGrey; color:black"|Films that can be examined | ||
|style="background:WhiteSmoke; color:black"| | |||
Any film that is transparent to the light in the given wavelength range | |||
e.g.: | |||
*Silicon Oxide | |||
*Silicon nitride | |||
*PolySilicon | |||
*Resists | |||
*Polymers | |||
*Very thin layers of metals | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
Any film that is transparent to the light in the given wavelength range | Any film that is transparent to the light in the given wavelength range | ||
| Line 67: | Line 98: | ||
|style="background:LightGrey; color:black"|Film thickness range | |style="background:LightGrey; color:black"|Film thickness range | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*~20Å to | *~20Å to a few micrometers (depending of the material) | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*~20Å to | *~20Å to a few micrometers (depending of the material) | ||
|style="background:WhiteSmoke; color:black"| | |||
*~20Å to a few micrometer (depending of the material) | |||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Process parameter range | !style="background:silver; color:black" align="center" valign="center" rowspan="4"|Process parameter range | ||
|style="background:LightGrey; color:black"|Wavelength range | |style="background:LightGrey; color:black"|Wavelength range | ||
|style="background:WhiteSmoke; color:black"| | |||
*210nm-1690nm | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*210nm-1690nm | *210nm-1690nm | ||
| Line 79: | Line 114: | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Incident angle range | |style="background:LightGrey; color:black"|Incident angle range | ||
|style="background:WhiteSmoke; color:black"| | |||
*45-90 degrees | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*45-90 degrees | *45-90 degrees | ||
| Line 85: | Line 122: | ||
|- | |- | ||
|style="background:LightGrey; color:black"|Beam size | |style="background:LightGrey; color:black"|Beam size | ||
|style="background:WhiteSmoke; color:black"| | |||
*3mm (spot size on sample depends on the angle) | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*2mm (spot size on sample depends on the angle) | *2mm (spot size on sample depends on the angle) | ||
| Line 92: | Line 131: | ||
|style="background:LightGrey; color:black"|Mapping facility | |style="background:LightGrey; color:black"|Mapping facility | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Can make | *Can make wafer maps on up to 150mm wafers | ||
|style="background:WhiteSmoke; color:black"| | |||
*Can make wafer maps on up to 150mm wafers | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*No mapping facility | *No mapping facility | ||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan=" | !style="background:silver; color:black" align="center" valign="center" rowspan="3"|Accessories | ||
|style="background:LightGrey; color:black"|Focusing optics | |style="background:LightGrey; color:black"|Focusing optics | ||
|style="background:WhiteSmoke; color:black"| | |||
*Focus lenses can be applied, reduces the beam diameter to 120µm | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Focus lenses can be applied, reduces the beam diameter to 125µm | *Focus lenses can be applied, reduces the beam diameter to 125µm | ||
| Line 107: | Line 150: | ||
*Extra stage for transmission measurements | *Extra stage for transmission measurements | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Base for ex-situ measurements, transmission data can be done by holding the sample up | *Extra stage for transmission measurements | ||
|style="background:WhiteSmoke; color:black"| | |||
*Base for ex-situ measurements, transmission data can be done by holding the sample up against the detector | |||
|- | |||
|style="background:LightGrey; color:black"|Heating stage | |||
|style="background:WhiteSmoke; color:black"| | |||
*Heating stage for measurements at temperatures up to 300C | |||
|style="background:WhiteSmoke; color:black"| | |||
*None | |||
|style="background:WhiteSmoke; color:black"| | |||
*None | |||
|- | |- | ||
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Substrates | !style="background:silver; color:black" align="center" valign="center" rowspan="2"|Substrates | ||
|style="background:LightGrey; color:black"|Batch size | |style="background:LightGrey; color:black"|Batch size | ||
|style="background:WhiteSmoke; color:black"| | |||
*One sample at a time smaller than 150mm (ask if you have anything larger) | |||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*One sample at a time smaller than 150mm (ask if you have anything larger) | *One sample at a time smaller than 150mm (ask if you have anything larger) | ||
| Line 120: | Line 175: | ||
*Any material that does not leave residuals on the stage and that does not evaporate | *Any material that does not leave residuals on the stage and that does not evaporate | ||
|style="background:WhiteSmoke; color:black"| | |style="background:WhiteSmoke; color:black"| | ||
*Any material that may go into the | *Any material that does not leave residuals on the stage and that does not evaporate | ||
|style="background:WhiteSmoke; color:black"| | |||
*Any material that may go into the ALD2 (when mounted on that system) | |||
|- | |- | ||
|} | |} | ||
| Line 128: | Line 185: | ||
==Filmtek 4000== | ==Filmtek 4000== | ||
[[image:Filmtek.JPG|275x275px|right|thumb|FilmTek 4000: positioned in cleanroom | {{CC-bghe2}} | ||
[[image:Filmtek.JPG|275x275px|right|thumb|FilmTek 4000: positioned in cleanroom D-1, {{photo1}}]] | |||
FilmTek 4000 is a computerized film thickness measurement and material characterization system. This system combines fiber-optic spectrophotometry with advanced material modeling software to provide an affordable and reliable tool for the simultaneous measurement of film thickness, index of refraction, and extinction coefficient | FilmTek 4000 is a computerized film thickness measurement and material characterization system. This system combines fiber-optic spectrophotometry with advanced material modeling software to provide an affordable and reliable tool for the simultaneous measurement of film thickness, index of refraction, and extinction coefficient | ||
| Line 138: | Line 196: | ||
'''The user manual, quality control procedure and results, technical information and contact information can be found in LabManager:''' | '''The user manual, quality control procedure and results, technical information and contact information can be found in LabManager:''' | ||
[http://labmanager | [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=169 FilmTek in LabManager] | ||
<br clear="all" /> | <br clear="all" /> | ||
| Line 192: | Line 250: | ||
<br clear="all" /> | <br clear="all" /> | ||
<!-- | |||
==Prism Coupler== | ==Prism Coupler== | ||
[[image:Prism_coupler.jpg|300x300px|right|thumb|Prism coupler: (old image), now positioned cleanroom D-3]] | [[image:Prism_coupler.jpg|300x300px|right|thumb|Prism coupler: (old image), now positioned cleanroom D-3]] | ||
| Line 260: | Line 319: | ||
|- | |- | ||
|} | |} | ||
--> | |||
<!-- | |||
==F10-RT reflectometer, transmitance, film thickness measurements == | |||
[[image:F10-RT.JPG|275x275px|right|thumb|F10-RT: positioned in basement project lab]] | |||
F10-RT is a combined reflectance and transmittance measurement system that can also use the reflectance measurements to get the film thickness of transparent thin films. This system combines fiber-optic spectrophotometry with material modeling software to provide an affordable tool for the measurement of reflectance, transmitance and film thickness. | |||
Reflectance and transmittance spectra can be obtained simultaneously. | |||
Normal incidence reflection data is collected and used to calculate thickness and index of refraction of the measured film. Absolute reflection data is obtained by comparing sample data to the measured reflection of a known reference sample. | |||
The spectrophotometer scans the sample over a predefined range of wavelengths. The software generates a reflection spectrum based on a previous measured reference scan, and then performs a regression on the unknown parameters to fit the simulated reflection. The resulting thin film parameters along with the measured and modeled spectra are then displayed for the user to examine. | |||
'''The user manual, quality control procedure and results, technical information and contact information can be found in LabManager:''' | |||
== | [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=466 F10-RT in LabManager] | ||
<br clear="all" /> | |||
===An overview of the performance of the F10-RT=== | |||
{| border="2" cellspacing="0" cellpadding="10" | |||
|- | |||
!style="background:silver; color:black;" align="left"|Purpose | |||
|style="background:LightGrey; color:black"|Reflectance, transmittance and film thickness measurements optically transparent thin films | |||
|style="background:WhiteSmoke; color:black"|[[:File:Filmetrics Datasheet - F10-RT b3M.pdf |See the datasheet here]] | |||
|- | |||
!style="background:silver; color:black" align="left"|Performance | |||
|style="background:LightGrey; color:black"|Thin film materials that can be measured||style="background:WhiteSmoke; color:black"| | |||
Reflectance: any flat surface larger than 6mm <br> | |||
Transmittance: any flat transparent material larger then 6mm <br> | |||
Thin film thickness: Any film that is transparent to the light in the given wavelength range | |||
ex: | |||
*Silicon Oxide | |||
*Silicon nitride | |||
*PolySilicon | |||
*Photoresists | |||
*SU8 | |||
*Other polymers | |||
*and many more | |||
|- | |||
|style="background:silver; color:black"| | |||
|style="background:LightGrey; color:black"|Film thickness range | |||
|style="background:WhiteSmoke; color:black"| | |||
*15 nm to 70 µm (depending of the material) | |||
*min 100nm (to measure n and k) | |||
|- | |||
|style="background:silver; color:black"| | |||
|style="background:LightGrey; color:black"|Probe spot size | |||
|style="background:WhiteSmoke; color:black"| | |||
*6 mm | |||
|- | |||
|style="background:silver; color:black"| | |||
|style="background:LightGrey; color:black"|Sample orientation | |||
|style="background:WhiteSmoke; color:black"| | |||
*Face down | |||
|- | |||
!style="background:silver; color:black" align="left"|Process parameter range | |||
|style="background:LightGrey; color:black"|Wavelength range | |||
|style="background:WhiteSmoke; color:black"| | |||
*380-1050 nm | |||
|- | |||
!style="background:silver; color:black" align="left"|Substrates | |||
|style="background:LightGrey; color:black"|Batch size | |||
|style="background:WhiteSmoke; color:black"| | |||
*One sample at a time - all sample larger than a diameter of 6 mm sizes up to 6" | |||
|- | |||
|style="background:silver; color:black"| | |||
| style="background:LightGrey; color:black"|Substrate material allowed | |||
|style="background:WhiteSmoke; color:black"| | |||
*In principle all materials as long as they do not leave residuals on the system | |||
|- | |||
|} | |||
--> | |||
<br clear="all" /> | |||
Latest revision as of 14:36, 2 September 2025
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
Comparison of the methods
For comparison of the methods for measuring optical constants and film thickness, see here: Film thickness and optical constants of optical transparent films
Ellipsometer RC2, Ellipsometer M2000XI (VASE) and Ellipsometer M-2000V
This section is written by Berit Herstrøm @ DTU Nanolab

The ellipsometer RC2 from J.A. Woollam Co., Inc is the newest of our ellipsometers. It performs slightly better then the M2000 and can measure the full Müller matrix. For most users the differences are very small. The ellipsometer VASE is actually a M2000XI-210 ellipsometer from J.A. Woollam Co., Inc.. We call it VASE (Variable Angle Spectroscopic Ellipsometry) because it can do spectroscopic ellipsometry at variable angles.
The ellipsometer M2000V is an in-situ ellipsometer from J.A. Wollam Co., Inc. This dedicated for being used on the Sputter System Lesker instrument or the ALD2 for in-situ measurements. When it is not on any system it is positioned next to the ALD2.
Ellipsometry is a very sensitive characterization technique which can be used to determine thin film layer thicknesses and/or optical constants. It sends in polarized light on the surface at different angles and measures the change in polarization state of the reflected light.
It is especially good for thin films in the thickness range of a few nanometers to a few microns. The layer should be transparent to light in the usable wavelength range for the thickness to be determined. Large roughness (>40nm) and features within the field of view can cause the measurement to fail.
Ellipsometry is an indirect measurement so a model has to be fit to the data in order to obtain the film thickness and optical constants. To learn more about ellipsometry you can take a look at the tutorial provided by the J. A. Woollam Co.
Access to use the CompleteEASE software can be found using Remote Desktop connection to: DTU-8CC0321MFL (you can only log on when you have the user competences in LabManager) or log on to https://remote.dtu.dk. There should be a connection via Citrix to DTU-8CC0321MFL. You will be prompted for user/password.
The user manuals, quality control procedure and results and contact information can be found in LabManager:
LabManager page for Ellipsometer RC2
LabManager page for Ellipsometer VASE
LabManager page for Ellipsometer M-2000V
More details
- Before training:
- First go through the Woollam short tutorial: tutorial
- Second watch our training video: Training Video
- To get more understanding - short intro from Quantum Design - Europe: [1] - optional
- Examples of advanced use of the ellipsometer
A rough overview of the performance of the Ellipsometers
| Equipment | Ellipsometer RC2 | Ellipsometer VASE (M2000XI) | Ellipsometer M-2000V | |
|---|---|---|---|---|
| Purpose |
|
|
| |
| Performance | Films that can be examined |
Any film that is transparent to the light in the given wavelength range e.g.:
|
Any film that is transparent to the light in the given wavelength range e.g.:
|
Any film that is transparent to the light in the given wavelength range e.g.:
|
| Film thickness range |
|
|
| |
| Process parameter range | Wavelength range |
|
|
|
| Incident angle range |
|
|
| |
| Beam size |
|
|
| |
| Mapping facility |
|
|
| |
| Accessories | Focusing optics |
|
|
|
| Transmission stage |
|
|
| |
| Heating stage |
|
|
| |
| Substrates | Batch size |
|
|
|
| Allowed materials |
|
|
| |
Filmtek 4000
Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
FilmTek 4000 is a computerized film thickness measurement and material characterization system. This system combines fiber-optic spectrophotometry with advanced material modeling software to provide an affordable and reliable tool for the simultaneous measurement of film thickness, index of refraction, and extinction coefficient
Normal incidence and polarized 70 degree reflection data is collected and used to calculate thickness and index of refraction of the measured film using SCI’s patented Differential Power Spectral Density (DPSD) technique. Absolute reflection data is obtained by comparing sample data to the measured reflection of a known reference sample, typically a silicon wafer with a thermally grown thin oxide (~63 nm) film.
The spectrophotometer scans the sample over a predefined range of wavelengths. The software generates a reflection spectrum based on a previously stored reference scan, and then performs a regression on the unknown parameters to fit the simulated reflection and power spectral density to the observed values. The resulting thin film parameters along with the measured and modeled spectra are then displayed for the user to examine.
The user manual, quality control procedure and results, technical information and contact information can be found in LabManager:
An overview of the performance of the FilmTek
| Purpose | Film thickness measurements and optical characterization of optically transparent thin films |
|
|---|---|---|
| Performance | Thin film materials that can be measured |
Any film that is transparent to the light in the given wavelength range ex:
|
| Film thickness range |
| |
| Process parameter range | Wavelength range |
|
| Substrates | Batch size |
|
| Substrate material allowed |
|