Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Chromium: Difference between revisions

Reet (talk | contribs)
Reet (talk | contribs)
 
(8 intermediate revisions by 3 users not shown)
Line 5: Line 5:
== Studies of Cr deposition processes ==
== Studies of Cr deposition processes ==


[[/Deposition of Chromium|Uniformity of Cr layers]] - ''Uniformity of Cr layers deposited with different methods and settings''
[[/Roughness of Chromium|Roughness of Chromium]] - ''Roughness and Uniformity of Cr layers deposited with different methods and settings''
 
[[/Sputtering of Cr in Wordentec|Sputtering of Cr in Wordentec]] - ''Settings and deposition rates''


[[/Sputtering of Cr in Sputter System (Lesker)|Sputtering of Cr in Sputter system (Lesker)]] - ''Settings and deposition rates''
[[/Sputtering of Cr in Sputter System (Lesker)|Sputtering of Cr in Sputter system (Lesker)]] - ''Settings and deposition rates''
Line 18: Line 16:


[[Specific_Process_Knowledge/Thin_film_deposition/Lesker/Stress_dependence_on_sputter_parameters_in_the_Lesker_sputter_system#Cr:_High_tensile_stress|Stress in sputtered Cr films]] - ''Extremely high tensile stress in Cr films deposited at high temperature''
[[Specific_Process_Knowledge/Thin_film_deposition/Lesker/Stress_dependence_on_sputter_parameters_in_the_Lesker_sputter_system#Cr:_High_tensile_stress|Stress in sputtered Cr films]] - ''Extremely high tensile stress in Cr films deposited at high temperature''


== Chromium deposition ==
== Chromium deposition ==
Chromium can be deposited by e-beam evaporation, thermal evaporation, and sputter deposition. It should be noted that in e-beam evaporation, chromium does not melt but evaporates directly from the solid phase. In the chart below you can compare the different deposition equipment. Further down you will find the results of some studies on chromium deposition.
Chromium can be deposited by e-beam evaporation, thermal evaporation, and sputter deposition. It should be noted that in e-beam evaporation, chromium does not melt but evaporates directly from the solid phase. In the chart below you can compare the different deposition equipment.  
 
{| border="1" cellspacing="0" cellpadding="4"  
{| border="1" cellspacing="0" cellpadding="4"  
   
   
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!
!
! E-beam evaporation E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]] and [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]])
! E-beam evaporation and sputter deposition ([[Specific Process Knowledge/Thin film deposition/Wordentec|Wordentec]])
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal evaporator]])
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal evaporator]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker sputterer]])
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker sputterer]])
Line 36: Line 31:
! General description
! General description
|E-beam deposition of Chromium
|E-beam deposition of Chromium
|E-beam and sputter deposition of Chromium
|Thermal deposition of Chromium
|Thermal deposition of Chromium
|Sputter deposition of Chromium
|Sputter deposition of Chromium
Line 44: Line 38:
! Pre-clean
! Pre-clean
|Ar ion gun (only in E-beam evaporator Temescal)
|Ar ion gun (only in E-beam evaporator Temescal)
|RF Ar clean
|
|
|RF Ar clean
|
|RF Ar clean
|RF Ar clean
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
! Layer thickness
! Layer thickness
|10Å to 1µm*
|10Å to 300 nm*
|10Å to 1µm*
|100 nm
|80 nm
|at least up to 200 nm
|at least up to 200 nm
|at least up to 200 nm
|at least up to 200 nm
Line 60: Line 52:
! Deposition rate
! Deposition rate
|1 Å/s to 10 Å/s
|1 Å/s to 10 Å/s
|1 Å/s to 10 Å/s (e-beam)
Sputtering: Depends on process parameters. See [[Specific Process Knowledge/Thin film deposition/Deposition of Chromium/Sputtering of Cr in Wordentec|here]] and process log.
|1 Å/s
|1 Å/s
|Depends on [[/Sputtering of Cr in Sputter System (Lesker)|process parameters]]. At least up to 1.48 Å/s. See process log.
|Depends on [[/Sputtering of Cr in Sputter System (Lesker)|process parameters]]. At least up to 1.48 Å/s. See process log.
Line 74: Line 64:
*3x8" wafers (ask for holder)
*3x8" wafers (ask for holder)
*Many smaller pieces
*Many smaller pieces
|
|
*24x2" wafers or
*Up to *3x 4" wafers or
*6x4" wafers or
*1x6" or 1x 8" wafer
*6x6" wafers
*Many smaller samples
|
*4x 2" wafer or
*1x 4" wafers or
*1x6" wafer or
*Several smaller pieces
*In theory up to 8" wafer (or 2x4" wafer) but uniformity will be bad
|
|
*1x6" wafers
*1x6" wafers
Line 98: Line 83:
|  
|  
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=511 cross-contamination sheet].
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=511 cross-contamination sheet].
|
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=167 cross-contamination sheet].
|
|
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=404 cross-contamination sheet].
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=404 cross-contamination sheet].
Line 115: Line 97:
! Comment
! Comment
| Takes approx. 20 min to pump down
| Takes approx. 20 min to pump down
| Takes approx. 1 hour to pump down
| Takes approx. 20 min to pump down
| Takes approx. 20 min to pump down
|
|
Line 123: Line 104:


|}  
|}  
'''*''' ''For thicknesses above 300 nm, please request permission from metal@nanolab.dtu.dk to ensure there is enough material.''
'''*''' ''For thicknesses above 300 nm, please request permission from metal@nanolab.dtu.dk to ensure there is enough material and to prioritize chamber cleaning as Cr tends to be a high-stress layer and thus causes flaking,''