Jump to content

Specific Process Knowledge/Characterization/XPS: Difference between revisions

Kare (talk | contribs)
Mmat (talk | contribs)
mNo edit summary
 
(79 intermediate revisions by 4 users not shown)
Line 1: Line 1:
{{Template:Author-jmli1}}


'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Characterization/XPS click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Characterization/XPS click here]'''
<!--Checked for updates on 14/5-2018 - ok/jmli -->




==The XPS tools at DTU Nanolab==


==XPS-ThermoScientific==
[[Image:XPS K-Alpha.jpg |thumb|x300px|The K-Alpha from 2007 is one of the first instruments of this type that was produced.{{photo1}} ]]
[[image:XPS instrument2.JPG|300x300px|right|thumb|The XPS system placed at Danchip (room 904, building 346).]]
[[Image:XPS Nexsa.png |thumb|x300px|The Nexsa from 2019 is on the surface very similar to the K-Alpha. Its panels, however, hide a whole range of supplementary techniques.{{photo1}} ]]


A X-ray Photoelectron Spectroscopy (XPS) system can be used at Danchip. The system is a Thermo K-Alpha system, placed in the basement of building 346.


In the basement under the cleanroom two X-ray Photoelectron Spectroscopy (XPS) systems are installed back-to-back in the center of room 904. They are both manufactured by Thermofisher and they enable the users to perform elemental and chemical analysis of samples. The [[Specific Process Knowledge/Characterization/XPS/K-Alpha |XPS K-Alpha]] is a base technique instrument providing XPS analysis. The [[Specific Process Knowledge/Characterization/XPS/Nexsa |XPS Nexsa]] is an upgraded version with all options.
* [[Specific Process Knowledge/Characterization/XPS/K-Alpha|The XPS K-Alpha page]]
* [[Specific Process Knowledge/Characterization/XPS/Nexsa|The XPS Nexsa page]]


==Elemental analysis==
The XPS instrument enables elemental analysis, chemical state analysis on the sample surface or deeper down by a depth profiling. A comparison about techniques and instruments used for elemental analysis at DTU Nanolab can be found on the page [[Specific Process Knowledge/Characterization/Element analysis|Element analysis]].
More about the different possibilities of the XPS instrument is found here:
*[[Specific Process Knowledge/Characterization/XPS/XPS technique|The XPS technique]]
*[[Specific Process Knowledge/Characterization/XPS/XPS elemental composition|Elemental analysis]]
*[[Specific Process Knowledge/Characterization/XPS/XPS Depth profiling|Depth profiling]]
*[[Specific Process Knowledge/Characterization/XPS/Carbon contamination|Carbon contamination]]


'''The user manual(s), user APV(s), technical information and contact information can be found in LabManager:'''
*[[Specific Process Knowledge/Characterization/XPS/ExtDocs | Links to external material ]]
<!-- remember to remove the type of documents that are not present -->
*[[Specific Process Knowledge/Characterization/XPS/Training | Links to instruction videos ]]


<!-- give the link to the equipment info page in LabManager: -->
== Getting access to the XPS tools==
[http://http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=276  XPS-ThermoScientific in LabManager]


==Elemental analysis==
Click [[Specific Process Knowledge/Characterization/XPS/Access | '''HERE''' ]] to see information on how to get access to the XPS.
The XPS instrument can be used to do elemental analysis, chemical state analysis on the sample surface or deeper down by a depth profiling. A comparison about techniques and instruments used for elemental analysis at Danchip can be found on the page [[Specific Process Knowledge/Characterization/Element analysis|Element analysis]].
 
== Analyzing XPS spectra ==
 
The analysis of XPS spectra is an art in itself. It can be done using various software packages available on the internet. In the links below we will focus on two such examples, Avantage and CasaXPS.
 
*[[Specific Process Knowledge/Characterization/XPS/SoftwareInstall|How to access XPS software: Download/install or by access to server]]
*[[Specific Process Knowledge/Characterization/XPS/Processing|Processing XPS data with Avantage]]
*[[Specific Process Knowledge/Characterization/XPS/Export2CasaXPS | Export Avantage data to CasaXPS]]


More about the different possibilities of the XPS instrument is found here:
==Techniques and option on the XPS tools==
*[[Specific Process Knowledge/Characterization/XPS/XPS technique|XPS technique]]
*[[Specific Process Knowledge/Characterization/XPS/XPS elemental composition|Elemental composition analysis]]
*[[Specific Process Knowledge/Characterization/XPS/XPS Chemical states |Chemical state analysis]]
*[[Specific Process Knowledge/Characterization/XPS/XPS Depth profiling|Depth profiling]]


==Equipment performance of XPS-ThermoScientific==
{| border="2" cellspacing="0" cellpadding="1"
|-
!style="background:silver; color:black;" align="left" colspan="2"|Equipment  
!style="background:silver; color:black;" align="left" |[[Specific Process Knowledge/Characterization/XPS/K-Alpha |XPS K-Alpha (Manufactured by Thermofisher)]]
!style="background:silver; color:black;" align="left" |[[Specific Process Knowledge/Characterization/XPS/Nexsa |XPS Nexsa (Manufactured by Thermofisher)]]
|-
!style="background:silver; color:black;" align="left" rowspan="2"|Purpose
|style="background:LightGrey; color:black"|Main
|style="background:WhiteSmoke; color:black"| XPS analysis using monochromated Al-Kα radiation at 1486.6 eV
|style="background:WhiteSmoke; color:black"| XPS analysis using monochromated Al-Kα radiation at 1486.6 eV
|-


{| border="2" cellspacing="0" cellpadding="20" |-
|style="background:LightGrey; color:black"|Alternative/complementary
!style="background:silver; color:black;" align="left"|Purpose
|style="background:LightGrey; color:black"|Chemical analysis
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
* [[Specific Process Knowledge/Characterization/XPS/XPS elemental composition|Probing elemental composition]]
* Work function measurements
* [[Specific Process Knowledge/Characterization/XPS/XPS Chemical states |Chemical state identification]]
|style="background:WhiteSmoke; color:black"|
* Non destructive technique
* Work function measurements
* Surface sensitive
* [[Specific Process Knowledge/Characterization/XPS/UPS technique| Ultraviolet Photoelectron Spectroscopy (UPS) with He I and He II UV source]]
* [[Specific Process Knowledge/Characterization/XPS/XPS Depth profiling|Depth profiling]] possible by ion beam etch of sample
* [[Specific Process Knowledge/Characterization/XPS/ISS|Ion Scattering Spectroscopy or ISS]]
* [[Specific Process Knowledge/Characterization/XPS/REELS|Reflected Electron Energy Loss Spectroscopy or REELS]]
* Angular Resolved Ultraviolet Photoelectron Spectroscopy (ARUPS)
* [[Specific Process Knowledge/Characterization/XPS/Raman|Raman spectroscopy]]
|-
|-
!rowspan="5" style="background:silver; color:black" align="left"| Performance
!rowspan="5" style="background:silver; color:black" align="left"| Performance
|style="background:LightGrey; color:black"|Spot size
|style="background:LightGrey; color:black"|Spot size
|style="background:WhiteSmoke; color:black"|Can be set between 30µm - 400µm
|style="background:WhiteSmoke; color:black"|XPS: 30µm - 400µm
|style="background:WhiteSmoke; color:black"|
* XPS: 10µm - 400µm
* Raman: > 15 µm
|-
|-
|style="background:LightGrey; color:black"|Probing depth
|style="background:LightGrey; color:black"|Pass energy
|style="background:WhiteSmoke; color:black"|Depending on probed element. Max probe depth lies within 10-200 Å.
|style="background:WhiteSmoke; color:black"|10-400 eV
|style="background:WhiteSmoke; color:black"|10-400 eV (XPS and ISS)
|-
|-
|style="background:LightGrey; color:black"|Resolution
|style="background:LightGrey; color:black"|Analysis modes
|style="background:WhiteSmoke; color:black"|Dependent on probed elements. Concentrations down to about 0,5 atomic % can in some cases be detected.
|style="background:WhiteSmoke; color:black"|Scanned and snapshot
|style="background:WhiteSmoke; color:black"|Scanned, snapshot and SnapMap
|-
|-
|style="background:LightGrey; color:black"|Charge compensation  
|style="background:LightGrey; color:black"|Charge compensation  
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"| Flood gun to be used for charge compensation of non conductive samples only
Flood gun can be used for charge compensation of non conductive samples
|style="background:WhiteSmoke; color:black"| Flood gun to be used for charge compensation of non conductive samples and for source of low energy electrons (REELS)
|-
|style="background:LightGrey; color:black"|Finding structures
|style="background:WhiteSmoke; color:black"|Choose measuring spot from camera image (magnified)
|-
|-
|-
|-
!rowspan="2" style="background:silver; color:black" align="left"|Depth profiling
|style="background:LightGrey; color:black"|Depth profiles
|style="background:LightGrey; color:black"|Purpose
|style="background:WhiteSmoke; color:black"|Depth profiles with single Ar ion bombardment
|style="background:WhiteSmoke; color:black"|With ion beam etch the top layer of the material can be removed, to do a depth profiling
* Monoatomic energy range 200-3000 eV
|-
|style="background:WhiteSmoke; color:black"|Depth profiles with MonoAtomic and Gas Cluster Ion Source ([[Media:MAGCIS.pdf |MAGCIS]])
|style="background:LightGrey; color:black"|Ion beam size
* Monoatomic energy range 200-4000 eV
|style="background:WhiteSmoke; color:black"| About 3x1 mm
* Cluster mode energy range: 2-8 keV
 
*Cluster size range: 75-2000 atoms
|-
|-
!rowspan="2" style="background:silver; color:black" align="left"|Substrates
!rowspan="2" style="background:silver; color:black" align="left"|Substrates / Samples
|style="background:LightGrey; color:black"|Substrate size
|style="background:LightGrey; color:black"|Sample holder size
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"| Maximum 60x60 mm
Maximum 60x60 mm
|style="background:WhiteSmoke; color:black"| Maximum 60x60 mm
|-
|-
| style="background:LightGrey; color:black"|Substrate thickness
| style="background:LightGrey; color:black"|Sample height
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"| Maximum 20 mm
Maximum height about 20 mm
|style="background:WhiteSmoke; color:black"| Maximum 20 mm
|-  
|-  
|}
|}
==Carbon Contamination==
--[[User:Kare|kare]] ([[User talk:Kare|talk]]) 09:29, 18 February 2015 (CET)
An unexpected carbon signal is often found in samples during XPS. The carbon typically originates from sample exposure to the air outside the XPS (e.g. the lab). Measurements of carbon contamination of a sputter cleaned Cu sample due to air exposure indicates that carbon contamination builds up to 20 At. % in approximately one minute.
[[File:AirCarbon.jpg]]
Measurements of the At. % of C on the Au-reference in the XPS after an initial sputter clean were conducted for 16 hours every hour. The results show that carbon is detectable after 1-2 hours and gradually builds up at a rate of approximately 0.6 At. percentage points per hour, i.e. much slower than if the sample is exposed to air. Thus carbon contamination on samples in the XPS typically originates from air exposure.
[[File:C-contamination.jpg]]