Jump to content

Specific Process Knowledge/Lithography/PMMA: Difference between revisions

From LabAdviser
Tigre (talk | contribs)
No edit summary
Elkh (talk | contribs)
No edit summary
 
(11 intermediate revisions by 3 users not shown)
Line 1: Line 1:
{{:Specific Process Knowledge/Lithography/authors_generic}}
'''Feedback to this page''': '''[mailto:lithography@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/PMMA click here]'''


{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%"
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" width="95%"
Line 4: Line 8:


|-
|-
|-style="background:silver; color:black"
|-style="background:black; color:white"
|'''Resist'''
|'''Resist'''
|'''Polarity'''
|'''Polarity'''
Line 26: Line 30:
| [http://www.allresist.com AllResist]
| [http://www.allresist.com AllResist]
|We have various types of PMMA in the cleanroom. Please contact [mailto:Lithography@danchip.dtu.dk Lithography] for information.
|We have various types of PMMA in the cleanroom. Please contact [mailto:Lithography@danchip.dtu.dk Lithography] for information.
|
| [[media:MSDS PMMA.pdf|MSDS PMMA]],  [[media:AR-P631_679.pdf|Processing guidelines]]
|See table <u>[[Specific_Process_Knowledge/Lithography/Coaters#Coaters:_Comparison_Table|here]] </u>
|See table <u>[[Specific_Process_Knowledge/Lithography/Coaters#Coaters:_Comparison_Table|here]] </u>
|Anisole
|Anisole
|MIBK:IPA (1:3), IPA:H2O
|IPA:H2O (7:3), MIBK:IPA (1:3)
|IPA
|IPA
|acetone/1165
|acetone/1165
|
|


|}
<br><br>


== Spin Curves ==
== Spin Curves ==




The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.  
The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers. Please notice, that the spinning curves were made in 2015.  




Line 55: Line 63:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!Spin Speed [rpm]
!Spin Speed [rpm]
!Acceleration [1/s2]
!Acceleration [rpm/s]
!Thickness [nm]
!Thickness [nm]
!St Dev
!St Dev
Line 98: Line 106:
|-style="background:silver; color:black" style="text-align:left;"  
|-style="background:silver; color:black" style="text-align:left;"  
!Spin Speed [rpm]
!Spin Speed [rpm]
!Acceleration [1/s2]
!Acceleration [rpm/s]
!Thickness [nm]
!Thickness [nm]
!St Dev
!St Dev

Latest revision as of 14:03, 5 May 2025

Specific Process Knowledge/Lithography/authors generic

Feedback to this page: click here


Resist Polarity Manufacturer Comments Technical reports Spinner Thinner Developer Rinse Remover Process flows (in docx-format)
PMMA Positive AllResist We have various types of PMMA in the cleanroom. Please contact Lithography for information. MSDS PMMA, Processing guidelines See table here Anisole IPA:H2O (7:3), MIBK:IPA (1:3) IPA acetone/1165




Spin Curves

The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers. Please notice, that the spinning curves were made in 2015.



AllResist AR-P 672.03 (PMMA) (~ 2ml per 4" wafer) spin coated on 'Spin Coater: Manual Standard Resists, E-5, WILTID & TIGRE, 26-10-2015. Softbake 3 min @ 150 degC.
Spin Speed [rpm] Acceleration [rpm/s] Thickness [nm] St Dev
4000 2000 95.55 0.55
5000 2000 85.50 0.92
7000 2000 72.79 1.18


AllResist AR-P 672.03 (PMMA) diluted 1:1 in Anisole (~ 2ml per 4" wafer) spin coated on 'Spin Coater: Manual Standard Resists, E-5, WILTID & TIGRE, 26-10-2015. Softbake 3 min @ 150 degC.
Spin Speed [rpm] Acceleration [rpm/s] Thickness [nm] St Dev
2000 2000 51.37 0.25
3000 2000 41.97 0.24
4000 2000 36.25 0.25
5000 2000 32.42 0.30
6000 2000 30.17 0.29
7000 2000 28.76 0.43