Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano121: Difference between revisions
Appearance
New page: == The nano1.21 recipe == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe nano1.21''' |- ! rowspan="6" align="center"| Recipe | Gas | C<sub>4</sub>F<sub>8</sub> 75 sccm, SF<su... |
No edit summary |
||
| (10 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
<!-- Ok, jmli 2020-0120 --> | |||
<!-- Page reviewed 9/8-2022 jmli --> | |||
<!--Checked for updates on 4/4-2025 - ok/jmli --> | |||
== The nano1.21 recipe == | == The nano1.21 recipe == | ||
<!-- revised 1/6-2015 by jmli --> | |||
{| border="2" cellpadding="2" cellspacing="1" | {| border="2" cellpadding="2" cellspacing="1" | ||
| Line 6: | Line 13: | ||
! rowspan="6" align="center"| Recipe | ! rowspan="6" align="center"| Recipe | ||
| Gas | | Gas | ||
| C<sub>4</sub>F<sub>8</sub> 75 sccm, SF<sub>6</sub> | | C<sub>4</sub>F<sub>8</sub> 75 sccm, SF<sub>6</sub> 38 sccm | ||
|- | |- | ||
| Pressure | | Pressure | ||
| Line 31: | Line 38: | ||
|- | |- | ||
| Mask | | Mask | ||
| | | 211 nm zep etched down to 74 nm | ||
|- | |- | ||
|} | |} | ||
<gallery caption="The results of the nano1. | <gallery caption="The results of the nano1.21 recipe" widths="250" heights="200" perrow="3"> | ||
image:WF_2E06_mar23B-030.jpg|The 30 nm trenches | image:WF_2E06_mar23B-030.jpg|The 30 nm trenches | ||
image:WF_2E06_mar23B-060.jpg|The 60 nm trenches | image:WF_2E06_mar23B-060.jpg|The 60 nm trenches | ||
| Line 44: | Line 51: | ||
C4F8 75 sccm, SF6 38 sccm, 4 mTorr, Strike 3 secs @ 15 mTorr, 800 W CP, 50 W PP, -10 degs, 120 secs | C4F8 75 sccm, SF6 38 sccm, 4 mTorr, Strike 3 secs @ 15 mTorr, 800 W CP, 50 W PP, -10 degs, 120 secs | ||
</gallery> | </gallery> | ||
{| {{table}} | |||
| align="center" style="background:#f0f0f0;"|'''Nominal trench line width''' | |||
| align="center" style="background:#f0f0f0;"|'''''' | |||
| align="center" style="background:#f0f0f0;"|'''30''' | |||
| align="center" style="background:#f0f0f0;"|'''60''' | |||
| align="center" style="background:#f0f0f0;"|'''90''' | |||
| align="center" style="background:#f0f0f0;"|'''120''' | |||
| align="center" style="background:#f0f0f0;"|'''150''' | |||
| align="center" style="background:#f0f0f0;"|'''Avg''' | |||
| align="center" style="background:#f0f0f0;"|'''Std''' | |||
|- | |||
| Etch rates||nm/min||168||182||185||189||191||183||9 | |||
|- | |||
| Sidewall angle||degs||91||91||91||91||90||91||0 | |||
|- | |||
| CD loss||nm/edge||7||-3||-3||-25||-26||-10||15 | |||
|- | |||
| CD loss foot||nm/edge||12||9||10||-11||1||4||9 | |||
|- | |||
| Bowing||||9||6||4||5||7||6||2 | |||
|- | |||
| Bottom curvature||||-47||-34||-34||-26||-19||-32||10 | |||
|- | |||
| zep||nm/min||||||||||||69|| | |||
|- | |||
| | |||
|} | |||
<!-- revised --> | |||