== The Sinano3.1 recipe ==
== The Sinano3.1 recipe ==
<!-- revised 1/6-2015 by jmli -->
<!-- revised 1/6-2015 by jmli -->
<!--Checked for updates on 4/4-2025 - ok/jmli -->
{| border="2" cellpadding="2" cellspacing="1"  
{| border="2" cellpadding="2" cellspacing="1"  
|+ '''Recipe Sinano3.1'''
|+ '''Recipe Sinano3.1'''

Latest revision as of 08:36, 4 April 2025

The Sinano3.1 recipe

Recipe Sinano3.1
Recipe Gas BCl3 3 sccm, HBR 17 sccm
Pressure 2 mTorr, Strike 3 secs @ 5 mTorr
Power 900 W CP, 50 W PP
Temperature 20 degs
Hardware 100 mm Spacers
Time 180 secs
Conditions Run ID 424, 425, 427, ID
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask The 180 nm zep resist etched down to 96 nm
Wafer WF_2B#2_feb06_2011



Nominal trench line width ' ' 30 60 90 120 150 Average Std. dev.
Etch rate nm/min 79 102 111 114 113 104 15
Sidewall angle degs 85 83 83 81 80 82 2
CD loss nm/edge -11 -11 -17 -9 -5 -11 5
CD loss foot nm/edge -11 -2 -2 9 16 2 11
Bowing 20 30 35 33 36 31 7
Bottom curvature -24 -18 -18 14 16 -6 19
Zep etch rate 30