Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinano35: Difference between revisions
Appearance
Created page with "== The Sinano3.5 recipe == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe Sinano3.5''' |- ! rowspan="6" align="center"| Recipe | Gas | BCl<sub>3</sub> 5 sccm, HB..." |
No edit summary |
||
| (6 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
<!--Checked for updates on 10/7-2019 - ok/jmli --> | |||
<!-- Ok, jmli 20170627 --> | |||
<!-- Ok, jmli 20170627 --> | |||
<!--Checked for updates on 24/8-2021. ok/ jmli--> | |||
<!--Checked for updates on 4/4-2025 - ok/jmli --> | |||
== The Sinano3.5 recipe == | == The Sinano3.5 recipe == | ||
<!-- revised 1/6-2015 by jmli --> | |||
{| border="2" cellpadding="2" cellspacing="1" | {| border="2" cellpadding="2" cellspacing="1" | ||
|+ '''Recipe Sinano3.5''' | |+ '''Recipe Sinano3.5''' | ||
| Line 31: | Line 37: | ||
|- | |- | ||
| Mask | | Mask | ||
| 180 nm zep etched down to 43 nm | | The [[Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/nanoetch/180nmzep|180 nm zep resist]] etched down to 43 nm | ||
|- | |- | ||
|} | |} | ||
Latest revision as of 08:36, 4 April 2025
The Sinano3.5 recipe
| Recipe | Gas | BCl3 5 sccm, HBR 15 sccm |
|---|---|---|
| Pressure | 5 mTorr, Strike 3 secs @ 5 mTorr | |
| Power | 900 W CP, 60 W PP | |
| Temperature | 20 degs | |
| Hardware | 100 mm Spacers | |
| Time | 120 secs | |
| Conditions | Run ID | 438, 440, ID |
| Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
| Mask | The 180 nm zep resist etched down to 43 nm |
- The results of the Sinano3.5 recipe
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches
| Nominal trench line width | ' | ' | 30 | 60 | 90 | 120 | 150 | Average | Std. dev. |
| Etch rate | nm/min | 90 | 109 | 112 | 114 | 117 | 108 | 11 | |
| Sidewall angle | degs | 83 | 81 | 82 | 81 | 80 | 81 | 1 | |
| CD loss | nm/edge | 27 | 47 | 62 | 80 | 97 | 63 | 27 | |
| CD loss foot | nm/edge | 27 | 47 | 62 | 80 | 97 | 63 | 27 | |
| Bowing | 10 | 14 | 13 | 11 | 13 | 12 | 2 | ||