Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinano35: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
 
(3 intermediate revisions by the same user not shown)
Line 1: Line 1:
<!--Checked for updates on 10/7-2019 - ok/jmli -->
<!-- Ok, jmli 20170627 -->
<!-- Ok, jmli 20170627 -->
<!-- Ok, jmli 20170627 -->
<!--Checked for updates on 24/8-2021. ok/ jmli-->
<!--Checked for updates on 4/4-2025 - ok/jmli -->
== The Sinano3.5 recipe ==
== The Sinano3.5 recipe ==
<!-- revised 1/6-2015 by jmli -->
<!-- revised 1/6-2015 by jmli -->

Latest revision as of 07:36, 4 April 2025


The Sinano3.5 recipe

Recipe Sinano3.5
Recipe Gas BCl3 5 sccm, HBR 15 sccm
Pressure 5 mTorr, Strike 3 secs @ 5 mTorr
Power 900 W CP, 60 W PP
Temperature 20 degs
Hardware 100 mm Spacers
Time 120 secs
Conditions Run ID 438, 440, ID
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask The 180 nm zep resist etched down to 43 nm


Nominal trench line width ' ' 30 60 90 120 150 Average Std. dev.
Etch rate nm/min 90 109 112 114 117 108 11
Sidewall angle degs 83 81 82 81 80 81 1
CD loss nm/edge 27 47 62 80 97 63 27
CD loss foot nm/edge 27 47 62 80 97 63 27
Bowing 10 14 13 11 13 12 2
Bottom curvature -24 -18 10 5 5 -4 15