== The Sinano3.6 recipe == | == The Sinano3.6 recipe == | ||
<!-- revised 1/6-2015 by jmli --> | <!-- revised 1/6-2015 by jmli --> | ||
Latest revision as of 08:34, 4 April 2025
The Sinano3.6 recipe
| Recipe | Gas | BCl3 5 sccm, HBR 15 sccm |
|---|---|---|
| Pressure | 10 mTorr, Strike 3 secs @ 5 mTorr | |
| Power | 900 W CP, 60 W PP | |
| Temperature | 20 degs | |
| Hardware | 100 mm Spacers | |
| Time | 180 secs | |
| Conditions | Run ID | 441, 442 ID |
| Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
| Mask | 190 nm zep etched down to 56 nm |
- The results of the Sinano3.6 recipe
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches
| Nominal trench line width | ' | ' | 30 | 60 | 90 | 120 | 150 | Average | Std. dev. |
| Etch rate | nm/min | 24 | 85 | 94 | 94 | 96 | 79 | 31 | |
| Sidewall angle | degs | 80 | 83 | 83 | 83 | 83 | 83 | 2 | |
| CD loss | nm/edge | -22 | -23 | -34 | -35 | -31 | -29 | 6 | |
| CD loss foot | nm/edge | -22 | -14 | -19 | -17 | -11 | -17 | 4 | |
| Bowing | 5 | 13 | 21 | 21 | 17 | 15 | 6 | ||
| Bottom curvature | -30 | -14 | -9 | 6 | 5 | -8 | 15 | ||
| Zep etch rate | 45 |