Specific Process Knowledge/Lithography/Strip: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Mbec (talk | contribs)
 
(20 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Strip click here]'''
{{cc-nanolab}}


[[Category: Equipment |Lithography strip]]
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Strip click here]'''
 
[[Category: Equipment|Lithography strip]]
[[Category: Lithography|Strip]]
[[Category: Lithography|Strip]]
__TOC__


= Strip Comparison Table =
= Strip Comparison Table =
{| border="2" cellspacing="0" cellpadding="2"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  


!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma asher|Plasma asher]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_1|Plasma Asher 1]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 2|Plasma Asher 2]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 2|Plasma Asher 2]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 3: Descum|Plasma Asher 3: Descum]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Strip#Plasma Asher 3: Descum|Plasma Asher 3: Descum]]</b>
Line 133: Line 137:
<br clear="all" />
<br clear="all" />


= Plasma ashing =
= Plasma Ashing =


{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
|-


{| border="2" cellspacing="0" cellpadding="4" align="left"
|-style="background:silver; color:black"
!
|
! Photoresist stripping
! Photoresist stripping
! [[Specific_Process_Knowledge/Lithography/Descum|Descum after lithography]]
! [[Specific_Process_Knowledge/Lithography/Descum|Descum after lithography]]
Line 143: Line 149:
! Ashing of organic material
! Ashing of organic material
|-  
|-  
|'''Process pressure'''
 
|-style="background:whitesmoke; color:black"
!Process pressure
|0.8- 1.2mbar
|0.8- 1.2mbar
|0.5- 1.0mbar  
|0.5- 1.0mbar  
Line 149: Line 157:
|0.8-1.5mbar
|0.8-1.5mbar
|-
|-
|'''Process gases'''
 
|-style="background:silver; color:black"
!Process gases
|
|
*O<sub>2</sub> (400 sccm)
*O<sub>2</sub> (400 sccm)
Line 159: Line 169:
|O<sub>2</sub>
|O<sub>2</sub>
|-
|-
|'''Process  power'''
 
|-style="background:whitesmoke; color:black"
!Process  power
|600-1000W
|600-1000W
|150-300W
|150-300W
Line 165: Line 177:
|1000W or less for heat- sensitive materials
|1000W or less for heat- sensitive materials
|-
|-
|'''Process  time'''
 
|-style="background:silver; color:black"
!Process  time
|5-60 minutes
|5-60 minutes
|1-5 minutes
|1-5 minutes
Line 171: Line 185:
|Between 0.5 and 20 hours, depending on the material
|Between 0.5 and 20 hours, depending on the material
|-
|-
|'''Batch size'''
 
|-style="background:whitesmoke; color:black"
!Batch size
|1-30
|1-30
|1-10
|1-10
Line 181: Line 197:
<br clear="all" />
<br clear="all" />


A typical process time for stripping of 1.5 µm AZ5214e resist is 15-25 min and for stripping of 9.5 µm AZ4562 resist is 20-35 min with the process parameters: 210 ml O<math>_2</math>/min or mixture of 210 ml O<math>_2</math>/min and 70 ml N<math>_2</math>/min, power 1000 W.


A Descum process in manual mode: O2: 70 sccm, N2: 70 sccm, power: 150 W, time: 10 min. Be sure to wait for cooling if the machine has been used at 1000W right before.
Typical process time for stripping in plasma asher 1 or 2:
At a load at 2 Fused silica wafers resist removed 0.01-01,5 um
*1.5 µm AZ 5214E resist film: ~15 min
*10 µm AZ 4562 resist film: ~45 min


==Plasma asher 1==
Typical process parameters:
*O<sub>2</sub>: 400 ml/min
*N<sub>2</sub>: 70 ml/min
*Power: 1000 W
 
 
A typical descum process in plasma asher 1 or 2:
*O<sub>2</sub>: 70 ml/min
*N<sub>2</sub>: 70 ml/min
*Power: 150 W
*Time : 10 min
 
 
Be sure to wait for chamber to cool down to room temperature, before runinng descum processes in plasma asher 1 or 2. At a load of 2 Fused silica wafers, the amount of resist removed will be 10 - 1500 nm.
 
'''NB: Use dedicated descum asher Plasma Asher 3: Descum for descumming.'''
 
==Plasma Asher 1==
[[Image:plasmaasher2.JPG|300x300px|thumb|The Plasma Asher 1 is placed in C-1]]
[[Image:plasmaasher2.JPG|300x300px|thumb|The Plasma Asher 1 is placed in C-1]]
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Strip#Plasma_asher click here]'''


The Plasma Asher 1 (TePla 300 auto load model) can be used for the following process:
The Plasma Asher 1 (TePla 300 auto load model) can be used for the following process:
Line 206: Line 237:
The machine can be used for almost every materials, but if you have any doubt about your materials are compatible with the plasma process it is better to ask photolithography group at Nanolab.
The machine can be used for almost every materials, but if you have any doubt about your materials are compatible with the plasma process it is better to ask photolithography group at Nanolab.


'''The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=55 LabManager]'''
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=55 LabManager] - '''requires login'''


===Process Information===
===Process Information===
Line 214: Line 245:
==Plasma Asher 2==
==Plasma Asher 2==
[[Image:Plasma_Asher_6inch.jpg|300x300px|thumb|Plasma asher for removing AZ resist on 6" wafers: positioned in E-5]]
[[Image:Plasma_Asher_6inch.jpg|300x300px|thumb|Plasma asher for removing AZ resist on 6" wafers: positioned in E-5]]
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_2 click here]'''


The Plasma Asher 2 is the same as Plasma Asher 1 but has another loading system which is more convenient for batch loading of 6inch substrates.  
The Plasma Asher 2 is the same as Plasma Asher 1 but has another loading system which is more convenient for batch loading of 6inch substrates.  
Line 240: Line 269:
The other materials have not been tested yet.
The other materials have not been tested yet.


'''The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=200 LabManager]'''
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=200 LabManager] - '''requires login'''


===Process Information===
===Process Information===
Line 250: Line 279:
==III-V Plasma Asher==
==III-V Plasma Asher==
[[Image:III-V_asher.jpg|300x300px|thumb|Plasma asher for removing resist on III-V samples: positioned in A-5]]
[[Image:III-V_asher.jpg|300x300px|thumb|Plasma asher for removing resist on III-V samples: positioned in A-5]]
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Strip#III-V_Plasma_Asher click here]'''


Diener Pico Plasma Asher for III-V materials.
Diener Pico Plasma Asher for III-V materials.


'''The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=186 LabManager]'''
The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=186 LabManager] - '''requires login'''


<br clear="all" />
<br clear="all" />
-->
-->
==Plasma Asher 3: Descum==
==Plasma Asher 3: Descum==
[[image:2017-03-15 13.12.45.jpg|350x350px|thumb|Plasma Asher 3: Descum is placed A-5]]
[[image:2017-03-15 13.12.45.jpg|350x350px|thumb|Plasma Asher 3: Descum is placed A-5]]
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_3 click here]'''


The Plasma Asher 3: Descum dedicated for resist descum i.e. removal of remains resist traces after development. It has a small chamber, so you can only load one 4 inch substrate ad time or few smaller pieces.
The Plasma Asher 3: Descum dedicated for resist descum i.e. removal of remains resist traces after development. It has a small chamber, so you can only load one 4 inch substrate ad time or few smaller pieces.
Line 278: Line 304:
The other materials have not been tested yet.
The other materials have not been tested yet.


'''The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=423 LabManager]'''
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=423 LabManager] - '''requires login'''


===Process Information===
===Process Information===
Line 288: Line 314:
==III-V Plasma Asher==
==III-V Plasma Asher==
[[Image:III-V_asher.jpg|300x300px|thumb|Plasma asher for removing resist on III-V samples: positioned in A-5]]
[[Image:III-V_asher.jpg|300x300px|thumb|Plasma asher for removing resist on III-V samples: positioned in A-5]]
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Strip#III-V_Plasma_Asher click here]'''


Diener Pico Plasma Asher for III-V materials.
Diener Pico Plasma Asher for III-V materials.


'''The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=186 LabManager]'''
The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=186 LabManager] - '''requires login'''


<br clear="all" />
<br clear="all" />
Line 299: Line 323:


=Resist Strip=
=Resist Strip=
 
[[Image:Resist_strip.jpg|300x300px|thumb|Resist strip bench in D-3]]
[[Image:Resist_strip.jpg|300x300px|thumb|Acetone strip bench in D-3]]
 
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Strip#Rough_and_Fine_Strip click here]'''


This resist strip is only for wafers without metal and SU-8.
This resist strip is only for wafers without metal and SU-8.
Line 314: Line 335:




'''The user manual and contact information can be found in LabManager: [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=385 Resist Strip]'''
The user manual and contact information can be found in LabManager: [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=385 Resist Strip] - '''requires login'''


<br clear="all" />
<br clear="all" />
Line 320: Line 341:
==Overview of wet bench 06 and 07==
==Overview of wet bench 06 and 07==


{| border="2" cellspacing="0" cellpadding="4" align="left"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
!
 
|-style="background:silver; color:black"
|
! [[Specific Process Knowledge/Lithography/Strip#Resist_Strip|Resist Strip]]  
! [[Specific Process Knowledge/Lithography/Strip#Resist_Strip|Resist Strip]]  
! [[Specific Process Knowledge/Lithography/LiftOff#Lift-off_wet_bench_07|Lift-off]]
! [[Specific Process Knowledge/Lithography/LiftOff#Lift-off_wet_bench_07|Lift-off]]
|-  
|-  
|'''General description'''
 
|
|-style="background:whitesmoke; color:black"
wet stripping of resist
!General description'''
|
|Wet stripping of resist
lift-off process
|Lift-off process
|-
|-
|'''Chemical solution'''
 
|-style="background:silver; color:black"
!Chemical solution
|NMP Remover 1165
|NMP Remover 1165
|NMP Remover 1165
|NMP Remover 1165
|-
|-
|'''Process temperature'''
|Up to 60°C
|Up to 60°C


|-style="background:whitesmoke; color:black"
!Process temperature
|Up to 65°C
|Up to 65°C
|-
|-


|'''Batch size'''
|-style="background:silver; color:black"
!Batch size
|
|
1 - 25 wafers
1 - 25 wafers
Line 348: Line 374:
1 - 25 wafers
1 - 25 wafers
|-
|-
|'''Size of substrate'''
 
|-style="background:whitesmoke; color:black"
!Size of substrate
|
|
*100 mm wafers
*100 mm wafers
Line 356: Line 384:
*150 mm wafers
*150 mm wafers
|-
|-
|'''Allowed materials'''
 
|-style="background:silver; color:black"
!Allowed materials
|
|
*Silicon
*Silicon
Line 362: Line 392:
*Silicon Nitride
*Silicon Nitride
*Silicon Oxynitride
*Silicon Oxynitride
|
|
*All metals except Type IV (Pb, Te)
All metals except Type IV (Pb, Te)
 
|-
|-
|}
|}

Latest revision as of 10:17, 18 March 2024

The contents on this page, including all images and pictures, was created by DTU Nanolab staff unless otherwise stated.

Feedback to this page: click here

Strip Comparison Table

Equipment Plasma Asher 1 Plasma Asher 2 Plasma Asher 3: Descum Resist strip Lift-off
Purpose

All purposes

Clean wafers only, no metal

Resist descum

Resist strip, no metal lift off

Lift-off

Method

Plasma ashing

Plasma ashing

Plasma ashing

Solvent and ultra sound

Solvent and ultra sound

Process parameters Process gasses
  • O2 (0 - 400 sccm)
  • N2
  • CF4
  • O2 (0 - 400 sccm)
  • N2
  • O2 (flow unknown)
  • NA
  • NA
Max. process power
  • 1000 W
  • 1000 W
  • 100% (power unknown)
  • NA
  • NA
Solvent
  • NA
  • NA
  • NA
  • NMP (Remover 1165)
  • Rinse in IPA
  • NMP (Remover 1165)
  • Rinse in IPA
Substrates Batch size
  • 1 small sample
  • 1 50 mm wafer
  • 1 - 30 100 mm wafers
  • 1 - 25 150 mm wafers
  • 1 small sample
  • 1 50 mm wafer
  • 1 - 30 100 mm wafers
  • 1 - 25 150 mm wafers
  • 1 small sample
  • 1 50 mm wafer
  • 1 100 mm wafer
  • 1 - 25 100 mm wafers
  • 1 - 25 150 mm wafers
  • 1 - 25 100 mm wafers
  • 1 - 25 150 mm wafers
Allowed materials
  • Silicon, glass, and polymer substrates
  • Film or pattern of all but Type IV

No metal allowed!

  • Silicon, glass, and polymer substrates
  • Film or pattern of photoresist/polymer
  • Silicon, III-V, and glass substrates
  • Film or pattern of all but Type IV

No metal allowed!

  • Silicon, glass, and polymer substrates
  • Film or pattern of photoresist/polymer
  • Silicon and glass substrates
  • Film or pattern of all but Type IV


Plasma Ashing

Photoresist stripping Descum after lithography Surface treatment of plastic, ceramic and metal Ashing of organic material
Process pressure 0.8- 1.2mbar 0.5- 1.0mbar 0.5- 1.0mbar 0.8-1.5mbar
Process gases
  • O2 (400 sccm)
  • N2 (0-70 sccm)
  • O2 (70-210 sccm)
  • N2 (0-70 sccm)
O2, CF4, N2 or their mixtures O2
Process power 600-1000W 150-300W 150-300W 1000W or less for heat- sensitive materials
Process time 5-60 minutes 1-5 minutes a few seconds to a few minutes Between 0.5 and 20 hours, depending on the material
Batch size 1-30 1-10 1 wafer at a time 1 wafer at a time, use a container, e.g Petri dish



Typical process time for stripping in plasma asher 1 or 2:

  • 1.5 µm AZ 5214E resist film: ~15 min
  • 10 µm AZ 4562 resist film: ~45 min

Typical process parameters:

  • O2: 400 ml/min
  • N2: 70 ml/min
  • Power: 1000 W


A typical descum process in plasma asher 1 or 2:

  • O2: 70 ml/min
  • N2: 70 ml/min
  • Power: 150 W
  • Time : 10 min


Be sure to wait for chamber to cool down to room temperature, before runinng descum processes in plasma asher 1 or 2. At a load of 2 Fused silica wafers, the amount of resist removed will be 10 - 1500 nm.

NB: Use dedicated descum asher Plasma Asher 3: Descum for descumming.

Plasma Asher 1

The Plasma Asher 1 is placed in C-1

The Plasma Asher 1 (TePla 300 auto load model) can be used for the following process:

  • Photoresist stripping
  • Descumming
  • Surface cleaning after storage
  • Surface cleaning after processes using oil pump or diffusion pump vacuum
  • Surface cleaning as part of photolithography after wet developing of lacquer structures prior to wet or plasma etching
  • Stripping of photoresist layers after etching, including after being exposed to high temperatures as after implantation, ion etching, sputter etching, RIE
  • Removal of organic passivation layers and masks
  • Etching of glass and ceramic
  • Etching of SiO, SiN, Si
  • Removal of polyimide layers

The machine can be used for almost every materials, but if you have any doubt about your materials are compatible with the plasma process it is better to ask photolithography group at Nanolab.

The user manual, user APV, and contact information can be found in LabManager - requires login

Process Information

Plasma Asher 2

Plasma asher for removing AZ resist on 6" wafers: positioned in E-5

The Plasma Asher 2 is the same as Plasma Asher 1 but has another loading system which is more convenient for batch loading of 6inch substrates.

In this machine, only O2 and N2 gases are used for processes (in PlasmaAsher1, CF4 is used as well).

The typical process parameters when operating the equipment:

  • Photeresist stripping

Pressure: 0.8 - 1.0 mbar

Gas: O2

Power: 600 - 1000 watts

Time: 5 -30 min., depending on photoresist type and thickness

A typical process time for stripping of 1.5 um AZ5214e resist is 25 min for 6 wafers load in a boat, recipe 18.

A Descum process in manual mode: O2:70, N2:70, power:150W, time:10 min

Be sure to wait for cooling if the mashine has been used at 1000W right before. At a load at 2 Fused silica wafers resist removed 0.01-01,5um

The other materials have not been tested yet.

The user manual, user APV, and contact information can be found in LabManager - requires login

Process Information



Plasma Asher 3: Descum

Plasma Asher 3: Descum is placed A-5

The Plasma Asher 3: Descum dedicated for resist descum i.e. removal of remains resist traces after development. It has a small chamber, so you can only load one 4 inch substrate ad time or few smaller pieces.

In this machine, only O2 and N2 gases are used for processes.

The typical process parameters when operating the equipment:

  • Photeresist descum

Pressure: 0.2 - 0.8mbar Gas: O2 Power: 50% - 100% Time: 1 -10 min., depending on photoresist type and thickness

The other materials have not been tested yet.

The user manual, user APV, and contact information can be found in LabManager - requires login

Process Information



Resist Strip

Resist strip bench in D-3

This resist strip is only for wafers without metal and SU-8.

There are one Remover 1165 bath for stripping and one IPA bath for rinsing.

Here are the main rules for resist strip use:

  • Place the wafers in a wafer holder and put them in the first bath for 10 min, this time is depending how much resist you have on the surface.
  • After the strip rinse your wafers in the IPA bath for 2-3 min.
  • Rinse your wafers for 4-5 min. in running water after stripping.


The user manual and contact information can be found in LabManager: Resist Strip - requires login


Overview of wet bench 06 and 07

Resist Strip Lift-off
General description Wet stripping of resist Lift-off process
Chemical solution NMP Remover 1165 NMP Remover 1165
Process temperature Up to 65°C Up to 65°C
Batch size

1 - 25 wafers

1 - 25 wafers

Size of substrate
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Allowed materials
  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride

All metals except Type IV (Pb, Te)