Specific Process Knowledge/Thin film deposition/Deposition of Silicon: Difference between revisions

From LabAdviser
Reet (talk | contribs)
No edit summary
Eves (talk | contribs)
No edit summary
 
(6 intermediate revisions by one other user not shown)
Line 13: Line 13:
*[[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_polysilicon/Deposition_of_polysilicon_using_LPCVD/Standard_recipes,_QC_limits_and_results_for_the_6%22_polysilicon_furnace|Deposition of polysilicon using the 6" polysilicon furnace]]
*[[Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_polysilicon/Deposition_of_polysilicon_using_LPCVD/Standard_recipes,_QC_limits_and_results_for_the_6%22_polysilicon_furnace|Deposition of polysilicon using the 6" polysilicon furnace]]


==Deposition of Silicon using PECVD==
At Nanolab you can also deposit silicon the using PECVD. The deposition temperature is 300 °C. 
* [[/Si deposition using PECVD|Si deposition using PECVD3]]


==Deposition of Silicon using sputter deposition==
==Deposition of Silicon using sputter deposition==


At Nanolab you can sputter silicon the using Wordentec or the Lesker Sputter systems. One of the advantages here is that you can deposit on almost any material you like.  
At Nanolab we can sputter silicon the using Wordentec or the Lesker Sputter systems. One of the advantages of sputtering is that you can deposit on almost any material you like.  


* [[Specific Process Knowledge/Thin film deposition/Si sputter in Wordentec|Si sputter deposition in the Wordentec]]
* [[Specific Process Knowledge/Thin film deposition/Si sputter in Wordentec|Si sputter deposition in the Wordentec]]
Line 23: Line 28:
* [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Metal-Oxide(PC3)|Si sputter deposition in the  Sputter-System Metal-Oxide(PC3)]]
* [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si sputter in Sputter-System Metal-Oxide(PC3)|Si sputter deposition in the  Sputter-System Metal-Oxide(PC3)]]


It was previosly possible to sputter Si with our [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300| IonFab 300]]. You can read about the deposition conditions and results from that [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300/IBSD of Si|here]].


Historical note: It was previosly possible to sputter Si with our [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300| IonFab 300]]. You can read about the deposition conditions and results from that [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300/IBSD of Si|here]].
==Deposition of Silicon using e-beam evaporation==
It is possible to e-beam evaporate silicon at Nanolab using the [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]]. As with sputtering you can deposit on almost any material. In e-beam evaporation the deposition is line-of-sight and will be suitable for lift-off. However for 8" wafers the system is not optimized for lift-off on the full diameter of the wafer.


==Deposition of Silicon using PECVD==
* [[Specific Process Knowledge/Thin film deposition/Deposition of Silicon/Si evaporation in E-beam evaporator Temescal-2|Si evaporation in E-beam evaporator (10-pockets)]]


At Nanolab you can also deposit silicon the using PECVD. The deposition temperature is 300 °C. 
* [[/Si deposition using PECVD|Si deposition using PECVD3]]


==Comparison of the methods for deposition of Silicon==
==Comparison of the methods for deposition of Silicon==
Line 42: Line 46:
! Sputter ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]])
! Sputter ([[Specific Process Knowledge/Thin film deposition/Lesker|Lesker]])
! Sputter ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]])
! Sputter ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]])
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]])
|-  
|-  
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
Line 51: Line 56:
| Sputter deposition of Si.  
| Sputter deposition of Si.  
| Sputter deposition of Si.  
| Sputter deposition of Si.  
| E-beam evaporation of Si.
|-
|-


Line 57: Line 63:
|Yes, B (boron) and P (phosphorus)
|Yes, B (boron) and P (phosphorus)
|Yes, B and P
|Yes, B and P
|None
|None
|None
|None
|None
Line 68: Line 75:
|RF Ar clean available
|RF Ar clean available
|RF Ar clean available
|RF Ar clean available
|None
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
Line 76: Line 84:
|few nm to >200 nm  
|few nm to >200 nm  
|few nm to ?
|few nm to ?
|few nm to 100 nm *
|-
|-


Line 88: Line 97:
| Depends on process parameters, roughly 0.2-2 Å/s. See Process Log.
| Depends on process parameters, roughly 0.2-2 Å/s. See Process Log.
|Depends on process parameters, at least 0.3 Å/s, see conditions [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|here]]
|Depends on process parameters, at least 0.3 Å/s, see conditions [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|here]]
| 1 Å/s
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
Line 93: Line 103:
|560 °C (amorphous) and 620 °C (poly)
|560 °C (amorphous) and 620 °C (poly)
|300 °C
|300 °C
|Wafers can be heated to 400 °C  
|room temperature
|Wafers can be heated to 600 °C  
|room temperature
 
|room temperature to 600 °C  
|room temperature to 250 °C  
|-
|-


Line 105: Line 116:
|Medium
|Medium
|Medium - may be possible to improve using HIPIMS
|Medium - may be possible to improve using HIPIMS
|no step coverage unless using tilt holder, in which case the step coverage can be very good and can be tuned.
|-
|-


Line 111: Line 123:
|Good for fused silica, silicon oxide, silicon nitride, silicon
|Good for fused silica, silicon oxide, silicon nitride, silicon
|Not tested, but do not deposit on top of silicon
|Not tested, but do not deposit on top of silicon
| 
| 
| 
| 
| 
Line 137: Line 150:
*Up to 10x6" or 4" wafers
*Up to 10x6" or 4" wafers
*many smaller pieces
*many smaller pieces
|
*Up to 4 x 6" wafer or
*3x 8" wafers (ask for special holder)
*Many smaller pieces


|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
Line 152: Line 169:
|
|
* Almost any that does not degas, see cross-contamination sheet
* Almost any that does not degas, see cross-contamination sheet
|
*Almost any that does not degas, see cross-contamination sheets
|
|
*Almost any that does not degas, see cross-contamination sheets
*Almost any that does not degas, see cross-contamination sheets
Line 169: Line 188:
|
|
*Almost any that does not degas, see the cross-contamination sheets
*Almost any that does not degas, see the cross-contamination sheets
|
*Almost any that does not degas, see cross-contamination sheet
|-
|-


Line 178: Line 200:
|  
|  
|
|
|  
|
| Please only deposit Si on the afternoon before a scheduled service as it can result in many flakes in the chamber. See the booking calendar or ask staff to find out when the next service will be.
|}
|}
'''*''' If you wish to deposit a thicker layer than 100 nm please talk to responsible staff or write to thinfilm@nanolab.dtu.dk

Latest revision as of 15:22, 7 February 2024

Feedback to this page: click here

Unless otherwise stated, this page is written by DTU Nanolab internal

PolySilicon can be deposited in several Nanolab tools. It can be sputtered, e-beam evaporated or be deposited in the PolySilicon furnaces. In the chart below you can compare the different deposition methods:


Deposition of PolySilicon using LPCVD

DTU Nanolab has two furnaces for deposition of LPCVD (Low Chemical Vapour Deposition) polysilicon: A 6" furnace (installed in 2011) for deposition of standard polySi, amorphous polySi and boron doped polySi on 100 mm or 150 mm wafers and a 4" furnace (installed in 1995) for deposition of standard polySi, amorphous polySi, boron- and phosphorous doped polySi on 100 mm wafers. In LabManager the two furnaces are named "Furnace: LPCVD Poly-Si (4") (B4)" and "Furnace: LPCVD Poly-Si (6") (E2)", respectively.

Deposition of Silicon using PECVD

At Nanolab you can also deposit silicon the using PECVD. The deposition temperature is 300 °C.

Deposition of Silicon using sputter deposition

At Nanolab we can sputter silicon the using Wordentec or the Lesker Sputter systems. One of the advantages of sputtering is that you can deposit on almost any material you like.

It was previosly possible to sputter Si with our IonFab 300. You can read about the deposition conditions and results from that here.

Deposition of Silicon using e-beam evaporation

It is possible to e-beam evaporate silicon at Nanolab using the E-beam evaporator (10-pockets). As with sputtering you can deposit on almost any material. In e-beam evaporation the deposition is line-of-sight and will be suitable for lift-off. However for 8" wafers the system is not optimized for lift-off on the full diameter of the wafer.


Comparison of the methods for deposition of Silicon

4" and 6" Furnace PolySi (Furnace LPCVD PolySi) PECVD (PECVD) Sputter (Wordentec) Sputter (Lesker) Sputter (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) E-beam evaporation (E-beam evaporator (10-pockets))
General description LPCVD (low pressure chemical vapour deposition) of a-Si and poly-Si Plasma Enhanced Chemical Vapor Deposition of Si Sputter deposition of Si. Sputter deposition of Si. Sputter deposition of Si. E-beam evaporation of Si.
Doping facility Yes, B (boron) and P (phosphorus) Yes, B and P None None None None
Pre-clean New wafers can go directly into the furnace. Processed wafers have to be RCA cleaned   RF Ar clean available RF Ar clean available RF Ar clean available None
Layer thickness ~5 nm to 2 µm, if thicker layers are needed please ask the furnace team. few nm to ~ 600 nm few nm to ~ 300 nm few nm to >200 nm few nm to ? few nm to 100 nm *
Deposition rate
  • undoped, boron doped:~100 Å/min
  • Phosphorous doped:~20 Å/min
~6 Å/s can probably be higher

On the order of 1 Å/s dependent on process parameters. See more here.

Depends on process parameters, roughly 0.2-2 Å/s. See Process Log. Depends on process parameters, at least 0.3 Å/s, see conditions here 1 Å/s
Process temperature 560 °C (amorphous) and 620 °C (poly) 300 °C room temperature room temperature room temperature to 600 °C room temperature to 250 °C
Step coverage Good Medium Medium Medium Medium - may be possible to improve using HIPIMS no step coverage unless using tilt holder, in which case the step coverage can be very good and can be tuned.
Adhesion Good for fused silica, silicon oxide, silicon nitride, silicon Not tested, but do not deposit on top of silicon        
Batch size
  • 1-30 wafers (4" furnace)
  • 1-25 wafes (6" furnace)
  • Several small samples
  • 1-2x 50 mm wafer
  • 1x 100 mm wafer
  • 1x 150 mm wafer
  • 24x 2" wafers or
  • 6x 4" wafers or
  • 6x 6" wafers
  • Up to 1x6" wafers
  • smaller pieces
  • Up to 10x6" or 4" wafers
  • many smaller pieces
  • Up to 4 x 6" wafer or
  • 3x 8" wafers (ask for special holder)
  • Many smaller pieces
Allowed substrates
  • Silicon wafers (new or RCA cleaned)
    • with layers of silicon oxide or silicon (oxy)nitride
    • from the A, B and E stack furnaces
  • Quartz/fused silica wafers (RCA cleaned)
  • See the cross contamination sheets
  • Almost any that does not degas.
  • Almost any that does not degas, see cross-contamination sheet
  • Almost any that does not degas, see cross-contamination sheets
  • Almost any that does not degas, see cross-contamination sheets
Allowed material *Only those above (under allowed substrates).
  • See the cross contamination sheets
  • Almost any that does not degas.
  • Almost any that does not degas, see the cross-contamination sheet
  • Almost any that does not degas, see the cross-contamination sheets
  • Almost any that does not degas, see cross-contamination sheet
Comment Only in PECVD3 Please only deposit Si on the afternoon before a scheduled service as it can result in many flakes in the chamber. See the booking calendar or ask staff to find out when the next service will be.

* If you wish to deposit a thicker layer than 100 nm please talk to responsible staff or write to thinfilm@nanolab.dtu.dk