Resist description

AZ MiR 701 is a positive UV photoresist. It is considered to have high selectivity for dry etching.

Spin coating

 
Spin curves for AZ MiR 701 (29 cps) using a 30 s spin-off, and a 60 s @ 90°C proximity softbake

Typical spin parameters:

  • Spin off: 30-60 s
  • Soft bake: 60 s @ 90°C in proximity


Exposure

Dehydration of resist film:
During exposure in the maskless aligners, MiR can be sensitive to dehydration by the air flow applied by the pneumatic auto-focus mechanism. This may lead to insufficient development, especially for small substrates. This problem can be alleviated by switching to the overview camera for a period of 1 minute before starting the exposure, or simply by parking the writehead away from the exposure location for 1 minute before starting the exposure. Dehydration can also mess up a dose test, but this can be fixed by increasing the spacing between the individual doses, or even better by extending the test design to 40mm or more in the Y-direction (adding a very small structure in the design file, or increasing the upper boarder during conversion).

The effect can also be reduced by increasing the soft bake.

Post-exposure bake

Typical PEB parameters:

  • PEB temperature: 110°C
  • PEB time: 60 s


During exposure, interaction between the incoming light and the light reflected by the substrate can cause a standing wave to form in the resist (especially true for single line/wavelength exposure). This leads to a wavy sidewall after development. The standing wave pattern can be reduced by introducing a post-exposure bake before development, which allows the activated PAC to diffuse into un-activated regions, thus smoothing the sidewall. The recommended PEB for MiR is 60 s at 110°C (for a 1 - 2 µm film). Thicker coatings may require longer bake, and substrate thickness and material may also affect the required baking time.

Since the post-exposure bake is at an elevated temperature compared to the soft bake, it will cause the resist film to become 5-10% thinner (probably due to continued evaporation of solvent). A 1.5 µm thick MiR resist film will be approximately 1.4 µm after PEB.

Development

Development speed:

  • Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min