The nano1.1 recipe

Recipe nano1.1
Recipe Gas C4F8 38 sccm, SF6 52 sccm
Pressure 4 mTorr, Strike 3 secs @ 15 mTorr
Power 600 W CP, 50 W PP
Temperature 10 degs
Hardware 100 mm Spacers
Time 120 secs
Conditions Run ID 1815
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask 1dfhj10 nm zep etched down to 6dgh4 nm