Jump to content

Specific Process Knowledge/Characterization/AFM: Atomic Force Microscopy/Workspaces

From LabAdviser

Feedback to this page: click here

What scanning mode, experiment/workspace and probe should I select

Roughness measurements Topographic measurements with no steep/abrupt steps Steep/abrupt steps but no high aspect ratio High aspect ratio measurements
Recommended mode Roughness measurement can be done in both Contact, Tapping and ScanAsyst mode. We recommend ScanAsyst mode because of less chance of (non-uniform) deformation of the sample and less tip wear - and because of ease of use. For Topographic measurements with no steep/abrupt steps we also recommend ScanAsyst mode due to less chance of (non-uniform) deformation of the sample and less tip wear - and because of ease of use. For Steep/abrupt steps but no high aspect ratio structures we still recommend ScanAsyst mode due to ease of use and lower top wear. For High aspect ratio measurements we recommend Tapping mode. There is not yet a ScanAsyst probe developed for high aspect ratio. Therefore we recommend Tapping mode.
Recommended probes ScanAsyst in air ScanAsyst in air ScanAsyst in air for ScanAsyst mode

TAP300Al-G for Tapping mode

AR5T-NCHR

FIB6-400A

Recommended experiment/Workspace

QNM in air*

QNM in air*

QNM in air* TappingMode 300nm trench (for steps <~1µm)

Tappping mode in air - 6µm Deep Trench (for steps >1~µm)

*By choosing the work space/experiment QNM in air (Mechanical properties - QNM in air) scanAsyst is included and so are the nanomechanical properties like modulus, adhesion, dissipation and deformation.


More information about de different modes

Contact, Tapping and Peak Force Tapping

Please flowing this link to Brukers homepage: Introduction_to_Brukers_ScanAsyst_and_PeakForce_Tapping_Atomic_Force_Microscopy_Technology_AFM_AN133.pdf

PeakForce tapping and quantitative nanomechanical mapping

Please flowing this link to Brukers homepage: PeakForce tapping and Nanomechanical option

Peak Force KPFM (Kelvin Probe Force Microscopy)

Please flowing this link to Brukers homepage: pf-kpfm.html

Evaluation of used probes

Box number and probe number User Initials Explanation SEM images Conclusion
Box1 no. 1 bghe A lot of triangles in the image    Tip end has broken off
Box1 no. 2 bghe/smurthy Round pillars became misshaped    Tip end has broken off or maybe if was not good to begin with
Box1 no. 3 bghe/zhongli Force curve bad, could not get the tip off the surface     Tip end has broken off
Box1 no. 4 mattod Used dirty sample, force curve very bad, tip probably broken   The hole cantilever has broken off
Box1 no. 5 mattod Tip broken during tip change   Tip/cantilever has been damaged
Box1 no. 6 abshir Bad force curve (fluctuates)     Tip end has broken off
Box1 no. 7 bghe Was OK on large structures but they got larger   
Box1 no. 8 mattod Bad force curve    Tip end has broken off
Box1 no. 9 kabi Blunt tip . Definitely (triangles)    Tip end has broken off
Box1 no. 10 kabi Blunt tip. Definitely (triangles)    Tip end has broken off
Box2 no. 1 mattod Bad force curve     Tip seems ok, or at least very close to okay
Box2 no. 2 mattod Broken tip     It looks like the tip end has been contaminated
Box2 no. 3 bghe Got large triangle scanning the tip checker   Tip end has broken off