Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/showerheadchange

From LabAdviser

Comparison of continuous processes

Process Before After
Name/Type Description Wafer ID Comment SEM images Wafer ID Comment SEM images
Continuous black silicon recipe on blank wafer 15 mins, -10 degrees, 32 mtorr, 60 sccm SF6, 55 sccm O2, 70 W platen S004592 Wafer centre   S004679 Wafer centre  
S004592 Wafer edge   S004679 Wafer edge  
S00XXX 8" wafer S00XXX Wafer centre File:S00XX centre.jpg
S00XXXx Wafer edge File:S00XXX dge.jpg S00XXX Wafer edge File:S00xxxx edge.jpg

Comparison of switched processes

Recipe description Name Temp. Deposition step Etch step Comments
Time Pres. C4F8 SF6 O2 Coil Time Pres. C4F8 SF6 O2 Coil Platen Showerhead Runs Key words
Polysilicon etch polySi etch DUV mask 30 2.3 10 50 0 0 600 5.0 10 20 60 5 400 40 Old 1 Slightly over-etching to ensure complete absence of grass
polySi etch DUV mask 30 2.3 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1
Cpoly1 30 1.2 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1 Very aggressive, unusable
Cpoly2 30 1.4 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1
Cpoly3 30 1.6 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1
Cpoly4 30 1.8 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1
Cpoly5 30 2.0 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1



Recipe description Name Temp. Deposition step Etch step Comments
Time Pres. C4F8 SF6 O2 Coil Time Pres. C4F8 SF6 O2 Coil Platen Showerhead Runs Key words
Polysilicon etch polySi etch DUV mask 30 2.3 10 50 0 0 600 5.0 10 20 60 5 400 40 Old 1 Slightly over-etching to ensure complete absence of grass
polySi etch DUV mask 30 2.3 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1
Cpoly1 30 1.2 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1 Very aggressive, unusable
Cpoly2 30 1.4 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1
Cpoly3 30 1.6 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1
Cpoly4 30 1.8 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1
Cpoly5 30 2.0 10 50 0 0 600 5.0 10 20 60 5 400 40 New 1