Specific Process Knowledge/Etch/DRIE-Pegasus/picoscope

From LabAdviser

Feedback to this page: click here

Process optimization using the Picoscope

The original standard recipes on Pegasus 1 differ in many ways. The second step of one of them is listed below:

Process A Step 2 parameters
Parameter Etch Dep
Gas flow (sccm) SF6 350 (1.5 s), 550 C4F8 200
Cycle time (secs) 7.0 4.0
Pressure (mtorr) 25 (1.5 s), 150 25
Coil power (W) 2800 2000
Platen power (W) 140 (1.5) 45 0
Common Temperature 20 degs

When running any recipe on the SPTS Pro software, a set of process parameters are recorded (defined in the logging recipe that can be modified like any other recipe) as the process runs. This data can be accessed later by looking up the datalog. During the process itself, one can also activate the 'Trace' to monitor the process parameters in real time. To the left in the figure below, some of the most important process parameters are shown for a process run of the recipe Process A.

One can see the multiplexing of the Bosch process by alternation of the gas flows of SF6 and C4F8


4 cycles of the recipe PrD4 recorded with the Picoscope
4 cycles of the recipe PrD4 recorded with the SPTS software
4 cycles of the recipe Prcocess A recorded with the Picoscope
4 cycles of the recipe PrD4 recorded with the SPTS software