Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using PECVD: Difference between revisions
No edit summary |
|||
| Line 6: | Line 6: | ||
=Recipes on PECVD2 for deposition of silicon oxides= | =Recipes on PECVD2 for deposition of silicon oxides= | ||
See [[Specific Process Knowledge/III-V Process/thin film dep/pecvd2| here]] | See [[Specific Process Knowledge/III-V Process/thin film dep/pecvd2| here]] | ||
==Quality control recipe== | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD2''' | |||
|- | |||
| | |||
*[http://labmanager.danchip.dtu.dk/d4Show.php?id=1988&mach=17 The QC procedure for PECVD2]<br> | |||
*[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=17 The newest QC data for PECVD2] | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:300px" | |||
! QC Recipe: | |||
! QCTOXIDE | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|12 sccm | |||
|- | |||
|N<sub>2</sub>O flow | |||
|710 sccm | |||
|- | |||
|N<sub>2</sub> flow | |||
|392 sccm | |||
|- | |||
|Pressure | |||
|550 mTorr | |||
|- | |||
|RF-power | |||
|100 W @380kHz | |||
|- | |||
|Deposition time | |||
|1 min | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
!QC limits | |||
!PECVD2 | |||
|- | |||
|Depostion rate of Silicon Oxide | |||
|69nm/min - 119nm/min | |||
|- | |||
|Non-uniformity of the deposition rate (std. deviation of 9 points) | |||
|0 - 2.8 nm | |||
|- | |||
|Refractive index of the Silicon Oxide | |||
|1.41 - 1.53 | |||
|- | |||
|Non-uniformity of the refrative index (std. deviation of 9 points) | |||
|0 - 0.07 | |||
|- | |||
|} | |||
|- | |||
|} | |||
|} | |||
==SiO2 Standard, High Rate== | |||
{| border="1" style="text-align: center; width: 400px; height: 150px;" | |||
! colspan="2" style="text-align: center;" style="background: #efefef;" | SiO2 Standard | |||
|- | |||
!N<math>_2</math>O-flow | |||
|1600 sccm | |||
|- | |||
!SiH<math>_4</math>-flow | |||
|17 sccm | |||
|- | |||
!RF-power (380 kHz) | |||
|380 W | |||
|- | |||
!Process Pressure | |||
|400 mTorr | |||
|- | |||
!Deposition rate | |||
|179 nm/min | |||
|- | |||
!index of refraction | |||
|1.461 | |||
|} | |||
==SiO2 Standard, Low Rate== | |||
{| border="1" style="text-align: center; width: 700px; height: 150px;" | |||
! colspan="2" style="text-align: left;" style="background: #efefef;" | 1STOxide | |||
! colspan="2" style="text-align: left;" style="background: #efefef;" | A test recipe | |||
|- | |||
!N<math>_2</math>-flow | |||
|392 sccm | |||
|392 sccm | |||
|- | |||
!N<math>_2</math>O-flow | |||
|1420 sccm (setting in software is 710 sccm) | |||
|1420 sccm (setting in software is 710 sccm) | |||
|- | |||
!SiH<math>_4</math>-flow | |||
|12 sccm | |||
|12 sccm | |||
|- | |||
!RF-power | |||
|100 W | |||
|150 W | |||
|- | |||
!Process Pressure | |||
|550 mTorr | |||
|700 mTorr | |||
|- | |||
!Deposition rate | |||
|~100 nm/min | |||
|109 ± 2 nm/min [tested: 2014-03-18] | |||
|- | |||
!index of refraction | |||
|1.47 | |||
|1.465 [tested: 2014-03-18] | |||
|- | |||
!Uniformity | |||
|<1 % | |||
|3.2% over the wafer [tested: 2014-03-18] | |||
|} | |||
===Deposition rate as a function of deposition time using 1STOxide:=== | |||
{| border="1" style="text-align: center; width: 400px; height: 150px;" | |||
|- | |||
| | |||
Deposition time [s] | |||
|Oxide thickness [nm] | |||
|Expected naturally grown oxide [nm] | |||
|Deposition rate [nm/min] | |||
|- | |||
|15 | |||
|26.9 | |||
|2 | |||
|99.6 | |||
|- | |||
|30 | |||
|51.9 | |||
|2 | |||
|99.8 | |||
|- | |||
|60 | |||
|102.4 | |||
|2 | |||
|100.4 | |||
|- | |||
|60 | |||
|102.7 | |||
|2 | |||
|100.7 | |||
|- | |||
|120 | |||
|201.1 | |||
|2 | |||
|99.6 | |||
|} | |||
===Thickness uniformity of test wafer using the test recipe=== | |||
[[image:PECVD2 SiO2 Test20 wafer map.jpg|350x350px|left|thumb|Thickness uniformity of test wafer using the test recipe.]] | |||
<br clear="all" /> | |||
==Silicon nitride== | |||
{| border="1" cellspacing="0" cellpadding="7" | |||
|- | |||
|Recipe name | |||
|SiH4 flow [sccm] | |||
|NH3 flow [sccm] | |||
|N2 flow [sccm] | |||
|Pressure [mTorr] | |||
|Power [W] | |||
|Description | |||
|- | |||
|1nitride | |||
|30 | |||
|20 | |||
|1000 | |||
|500 | |||
|80 | |||
| | |||
|- | |||
|} | |||
=Recipes on PECVD3 for deposition of silicon oxides= | =Recipes on PECVD3 for deposition of silicon oxides= | ||
Revision as of 09:07, 6 May 2014
Feedback to this page: click here
At the moment DANCHIP has 2(3) PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 has been decommissioned and PECVD3 are for silicon based processing allowing wafers with small abount of metal (<5% wafer coverage). PECVD2 is clean wafers both for silicon based materials and for III-V materials. At the moment PECVD2 is described under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD2 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
Recipes on PECVD2 for deposition of silicon oxides
See here
Quality control recipe
| Quality Controle (QC) for PECVD2 | ||||||||||||||||||||||||||
|
SiO2 Standard, High Rate
| SiO2 Standard | |
|---|---|
| NO-flow | 1600 sccm |
| SiH-flow | 17 sccm |
| RF-power (380 kHz) | 380 W |
| Process Pressure | 400 mTorr |
| Deposition rate | 179 nm/min |
| index of refraction | 1.461 |
SiO2 Standard, Low Rate
| 1STOxide | A test recipe | ||
|---|---|---|---|
| N-flow | 392 sccm | 392 sccm | |
| NO-flow | 1420 sccm (setting in software is 710 sccm) | 1420 sccm (setting in software is 710 sccm) | |
| SiH-flow | 12 sccm | 12 sccm | |
| RF-power | 100 W | 150 W | |
| Process Pressure | 550 mTorr | 700 mTorr | |
| Deposition rate | ~100 nm/min | 109 ± 2 nm/min [tested: 2014-03-18] | |
| index of refraction | 1.47 | 1.465 [tested: 2014-03-18] | |
| Uniformity | <1 % | 3.2% over the wafer [tested: 2014-03-18] | |
Deposition rate as a function of deposition time using 1STOxide:
|
Deposition time [s] |
Oxide thickness [nm] | Expected naturally grown oxide [nm] | Deposition rate [nm/min] |
| 15 | 26.9 | 2 | 99.6 |
| 30 | 51.9 | 2 | 99.8 |
| 60 | 102.4 | 2 | 100.4 |
| 60 | 102.7 | 2 | 100.7 |
| 120 | 201.1 | 2 | 99.6 |
Thickness uniformity of test wafer using the test recipe

Silicon nitride
| Recipe name | SiH4 flow [sccm] | NH3 flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| 1nitride | 30 | 20 | 1000 | 500 | 80 |
Recipes on PECVD3 for deposition of silicon oxides
| Quality Controle (QC) for PECVD3 - oxide | ||||||||||||||||||||||
|
Recipes
| Recipe name | SiH4 flow [sccm] | N2O flow [sccm] | N2 flow [sccm] | B2H6 flow [sccm] | PH3 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| LFSiO | 12 | 1420 | 392 | 0 | 0 | 550 | 60 | Uniform silicon oxide |
| 1PBSG | 17 | 1600 | 0 | 135 | 40 | 500 | 800LF | BPSG glass for waveguide cladding layer |
LF=Low Frequency
Expected results
| Recipe name | Deposition rate [nm/min] | RI | Uniformity [%] |
| LFSiO | ~75 | ~1.48 | <1 |
| 1PBSG | ~228 nm/min | . | ~17% |
Recipes on PECVD3 for deposition of doped oxide
Recipes
| Recipe name | SiH4 flow [sccm] | N2O flow [sccm] | N2 flow [sccm] | GeH4 flow [sccm] (scaled by 100) | B2H6 flow [sccm] | PH3 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| Core-Ge | 17 | 1600 | 300 | 300 | 0 | 0 | 400 | 600 LF | Process for germanium doped core layer developed by Haiyan Ou from DTU Photonics
Annnealing: Anneal bond furnace, recipe "core1100" |
| Top-BPSG | 17 | 1600 | 0 | 0 | 100 | 40 | 500 | 800 LF | Process for PBSG top clading layer developed by Haiyan Ou from DTU Photonics
Annnealing/oxidation: Anneal bond furnace, recipe "clad1000" |
Expected results
| Recipe name | Deposition rate [nm/min] | Refractive index |
| Core-Ge | ~188 nm/min | ~1.46969 |
| Top-BPSG | ~248 nm/min | ~1.458 |
Recipes on PECVD1 for deposition of silicon oxides Expired!
Recipes
| Recipe name | SiH4 flow [sccm] | N2O flow [sccm] | N2 flow [sccm] | B2H6 flow [sccm] | PH3 flow [sccm] | GeH4*100 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| 1oxide/1ox_std/standard | 17 | 1600 | 0 | 0 | 0 | 0 | 400 | 380LF | Process control recipe. Developed for waveguides |
| 1PBSG | 17 | 1600 | 0 | 135 | 40 | 0 | 500 | 800LF | Developed for waveguide top cladding by Haiyan Ou @DTU Photonics'. |
| BGE_PBSG | 17 | 1600 | 0 | 240 | 60 | 0 | 500 | 800LF | Low stress PBSG |
| HO_core | 17 | 1600 | 300 | 0 | 0 | 400 | 400 | 600LF | Developed by Haiyan Ou @fotonik@dtu |
| HO_top | 17 | 1600 | 0 | 107 | 40 | 0 | 500 | 800LF | Developed by Haiyan Ou @fotonik@dtu |
Expected results
| Recipe name | Deposition rate [µm/min] | RI | Uniformity [%] | Comments |
| 1oxide/1ox_std/standard | ~0.193 | 1.46 | 2 | The latest measured values can be seen in the process control sheet in LabManager |
| 1PBSG | ~0.3 | 1.458@633nm |