=Recipes on PECVD3 for deposition of silicon oxides=
=Recipes on PECVD3 for deposition of silicon oxides=
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD3 - oxide'''
|-
|
*[http://labmanager.danchip.dtu.dk/d4Show.php?id=1389&mach=18 The QC procedure for RIE1 and RIE2]<br>
*[http://www.labmanager.danchip.dtu.dk/view_binary.php?type=data&mach=18 The newest QC data for RIE1]<br>
*[http://www.labmanager.danchip.dtu.dk/view_binary.php?type=data&mach=19 The newest QC data for RIE2]
{| {{table}}
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:200px"
! QC Recipe:
! QCOXIDE
|-
| SF<sub>6</sub> flow
|32 sccm
|-
|O<sub>2</sub> flow
|8 sccm
|-
|Pressure
|80 mTorr
|-
|RF-power
|30 W
|-
|Etch Load
|50%
|-
|}
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
!QC limits
!RIE1
!RIE2
|-
|Etch rate in Si
|0.2 - 0.6 µm/min
|0.2 - 0.6 µm/min
|-
|Non-uniformity
|2 - 5 %
|2 - 5 %
|-
|}
|-
|}
|}
===Recipes===
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
{| border="1" cellspacing="0" cellpadding="7"

Revision as of 10:23, 26 November 2013

Feedback to this page: click here


At the moment DANCHIP has 2(3) PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 has been decommissioned and PECVD3 are for silicon based processing allowing wafers with small abount of metal (<5% wafer coverage). PECVD2 is clean wafers both for silicon based materials and for III-V materials. At the moment PECVD2 is described under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD2 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.

Recipes on PECVD2 for deposition of silicon oxides

See here

Recipes on PECVD1 for deposition of silicon oxides

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] GeH4*100 flow [sccm] Pressure [mTorr] Power [W] Description
1oxide/1ox_std/standard 17 1600 0 0 0 0 400 380LF Process control recipe. Developed for waveguides
1PBSG 17 1600 0 135 40 0 500 800LF Developed for waveguide top cladding by Haiyan Ou @DTU Photonics'.
BGE_PBSG 17 1600 0 240 60 0 500 800LF Low stress PBSG
HO_core 17 1600 300 0 0 400 400 600LF Developed by Haiyan Ou @fotonik@dtu
HO_top 17 1600 0 107 40 0 500 800LF Developed by Haiyan Ou @fotonik@dtu

Expected results

Recipe name Deposition rate [µm/min] RI Uniformity [%] Comments
1oxide/1ox_std/standard ~0.193 1.46 2 The latest measured values can be seen in the process control sheet in LabManager
1PBSG ~0.3 1.458@633nm

Recipes on PECVD3 for deposition of silicon oxides

Quality Controle (QC) for PECVD3 - oxide
QC Recipe: QCOXIDE
SF6 flow 32 sccm
O2 flow 8 sccm
Pressure 80 mTorr
RF-power 30 W
Etch Load 50%
QC limits RIE1 RIE2
Etch rate in Si 0.2 - 0.6 µm/min 0.2 - 0.6 µm/min
Non-uniformity 2 - 5 % 2 - 5 %

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
LFSiO 12 1420 392 0 0 550 60 Uniform silicon oxide
1PBSG 17 1600 0 135 40 500 800LF BPSG glass for waveguide cladding layer

LF=Low Frequency

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%]
LFSiO ~75 ~1.48 <1
1PBSG ~228 nm/min . ~17%

Recipes on PECVD3 for deposition of doped oxide

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] GeH4 flow [sccm] (scaled by 100) B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
Core-Ge 17 1600 300 300 0 0 400 600 LF Process for germanium doped core layer developed by Haiyan Ou from DTU Photonics

Annnealing: Anneal bond furnace, recipe "core1100"

Top-BPSG 17 1600 0 0 100 40 500 800 LF Process for PBSG top clading layer developed by Haiyan Ou from DTU Photonics

Annnealing/oxidation: Anneal bond furnace, recipe "clad1000"

Expected results

Recipe name Deposition rate [nm/min] Refractive index
Core-Ge ~188 nm/min ~1.46969
Top-BPSG ~248 nm/min ~1.458