Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using PECVD: Difference between revisions

From LabAdviser
Line 30: Line 30:
|RI
|RI
|Uniformity [%]
|Uniformity [%]
|
|-  
|-  
|1oxide
|1oxide
Line 36: Line 35:
|1.46
|1.46
|2
|2
|
|-
|-
|}
|}


==Recipes on PECVD3 for deposition of silicon oxides==
==Recipes on PECVD3 for deposition of silicon oxides==

Revision as of 15:58, 28 November 2007

At the moment DANCHIP has 3 PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.

Recipes on PECVD1 for deposition of silicon oxydes

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
1oxide

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%]
1oxide 193 1.46 2

Recipes on PECVD3 for deposition of silicon oxides

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
LFSiO 12 1420 392 550 60

LF=Low Frequency

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%]
LFSiO ~81 ~1.48 <1