Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using LPCVD TEOS: Difference between revisions
No edit summary |
No edit summary |
||
| Line 2: | Line 2: | ||
constant of 3.56 (For thermal oxide it is 3.46). Furthermore TEOS has a breakdown | constant of 3.56 (For thermal oxide it is 3.46). Furthermore TEOS has a breakdown | ||
voltage in the order of <math> 10^6 </math> | voltage in the order of <math> 10^6 </math> | ||
Danchip have two [[Specific Process Knowledge/Thin film deposition/B2 Furnace LPCVD Nitride|LPCVD furnaces]] for deposition of silicon nitride: A new furnace (installed in 2008) for deposition of stoichiometric nitride on 4" and 6" wafers and an older furnace (installed in 1995) for deposition of stoichiometric nitride and low stress nitride on 4" wafers. Please, be aware that it is not allowed to deposit low stress nitride i the new nitride furnace (to avoid problems with particles). | |||
On the new LPCVD nitride furnace there are two standard processes for deposition of stoichiometric nitride, one for 4" wafers called "4NITDAN" and one for 6" wafers called "6NITDAN". The old LPCVD nitride furnace is mainly dedicated for deposition of low stress nitride, which does affect the cleanliness of the furnace, but stoichiometric nitride can also be deposited in the furnace. On this furnace the process for stoichiometric nitride is called "NITRIDE", and the process for low stress nitride (silicon rich nitride) is called "SIRICH" | |||
==Process parameters for the two standard deposition recipes on the old nitride furnace:== | |||
{| border="2" cellspacing="1" cellpadding="5" | |||
!Recipe name | |||
!Wafer size and number of wafers | |||
!Temperature [<sup>o</sup>C] | |||
!Pressure [mTorr] | |||
!NH3 gas flow [sccm] | |||
!DCS gas flow [sccm] | |||
!Comments | |||
|- | |||
|"NITRIDE" | |||
|4" wafers | |||
1-35 wafers in a run | |||
|800 - 825 | |||
|230 | |||
|75 | |||
|25 | |||
|Stoichiometric nitride | |||
|- | |||
|"SIRICH" | |||
|4" wafers | |||
1-35 wafers in a run | |||
|835 | |||
|112 | |||
|13 | |||
|93 | |||
|Low stress nitride (silicon rich nitride) | |||
This was first tested at DTU Danchip by Matthias Heschel,<br \> ''M. Heschel and S. Bouwstra "Robust, compliant silicon nitride membranes", Proceedings MME '95, Copenhagen, Denmark, September 1995, pp. 84-87'' | |||
|} | |||
==Expected results when using the two standard recipes on the old nitride furnace:== | |||
These are typical values | |||
{| border="2" cellspacing="1" cellpadding="6" | |||
!Recipe name | |||
!Deposition rate [Å/min] | |||
!Refractive index@630nm | |||
!Thickness variation on wafer | |||
!Thickness variation along the boat | |||
!Stress [MPa] | |||
|- | |||
|"NITRIDE" | |||
|46-52 | |||
|2.01-2.02 | |||
|<1.3% | |||
|<4% | |||
|1000 | |||
|- | |||
|"SIRICH" | |||
|30-40 | |||
|2.20-2.30 | |||
|<5% | |||
|<20% | |||
|(-50 to 50) | |||
|- | |||
|} | |||
==Process parameters for the two standard deposition recipes on the new nitride furnace:== | |||
{| border="2" cellspacing="1" cellpadding="5" | |||
!Recipe name | |||
!Wafer size and number of wafers | |||
!Temperature [<sup>o</sup>C] | |||
!Pressure [mTorr] | |||
!NH3 gas flow [sccm] | |||
!DCS gas flow [sccm] | |||
!Comments | |||
|- | |||
|"4NITDAN" | |||
|4" wafers | |||
1-25 wafers in a run | |||
|780 - 790 | |||
|200 | |||
|100 | |||
|33 | |||
|Stoichiometric nitride | |||
|- | |||
|"6NITDAN" | |||
|6" wafers | |||
1-25 wafers in a run | |||
|780 - 790 | |||
|200 | |||
|120 | |||
|30 | |||
|Stoichiometric nitride | |||
|} | |||
==Expected results when using the two standard recipes on the new nitride furnace:== | |||
These are typical values | |||
{| border="2" cellspacing="1" cellpadding="6" | |||
!Recipe name | |||
!Deposition rate [Å/min] | |||
!Refractive index@630nm | |||
!Thickness variation on wafer | |||
!Thickness variation along the boat | |||
!Stress [MPa] | |||
|- | |||
|"4NITDAN" | |||
|~ 30-35 | |||
|2.00 - 2.01 | |||
|<3% | |||
|<3% | |||
| | |||
|- | |||
|"6NITDAN" | |||
|~ 30-35 | |||
|2.00 - 2.01 | |||
|<3% | |||
| | |||
|- | |||
|} | |||
==Using LPCVD silicon nitride as a masking material for KOH etching== | |||
At Danchip stoichiometric silicon nitride is mainly used as masking material for potassium hydroxide (KOH) etching. The etch rate of the nitride in 80 <sup>o</sup>C KOH is expected to be less than 1 Å/min. | |||
There are regularly users having problems with pinholes in the silicon nitride after KOH etching. It is not always clear what the reasons are, but we suspect problems can arise due to | |||
*too many or too large particles in the nitride. | |||
*too rough handling of the wafers after the nitride deposition. | |||
*too much stress between the nitride and the underlying layer. | |||
===Our recommendations to try and avoid pinhole problems are:=== | |||
'''To avoid too many or too large particles in the nitride'''<br\> | |||
*Use the new nitride furnace, if you have to deposit stoichiometric nitride. In order to avoid problems with particles it is not allowed to deposit low stress nitride in this furnace, and the particles level is therefore low compared to the older nitride furnace | |||
*Before running a process keep in close contact with the Danchip staff (especially the process specialist on the furnace) or take a look at the logbook to make sure that the nitride furnace is expected to be in a good state. | |||
'''To avoid too rough handling of the wafers after the nitride deposition'''<br\> | |||
*After the deposition handle the wafers with a clean glove on the edge of the wafers (no tweezers). | |||
*Be careful not to scratch wafers with nitride (e.g. up against each other or on the spinner or the aligner). | |||
*If you have nitride on the back side of a wafer while aligning, consider if you can protect it with e.g. a photoresist layer before loading it onto the aligner. Or use a non-vacuum aligner chuck with a big hole in the middle, so that the wafer is only laying on the edge. Avoid hard contact in the aligner if possible. | |||
'''To avoid too much stress between the nitride and the underlying layer'''<br\> | |||
*It is recommended to have a of silicon oxide layer between the silicon substrate and the nitride layer to reduce the stress level between the layers. The silicon nitride is then expected to have less tendency to break. | |||
for sjov | for sjov | ||
Revision as of 12:49, 26 January 2009
TEOS oxide, has a dielectric constant of 3.56 (For thermal oxide it is 3.46). Furthermore TEOS has a breakdown voltage in the order of
Danchip have two LPCVD furnaces for deposition of silicon nitride: A new furnace (installed in 2008) for deposition of stoichiometric nitride on 4" and 6" wafers and an older furnace (installed in 1995) for deposition of stoichiometric nitride and low stress nitride on 4" wafers. Please, be aware that it is not allowed to deposit low stress nitride i the new nitride furnace (to avoid problems with particles).
On the new LPCVD nitride furnace there are two standard processes for deposition of stoichiometric nitride, one for 4" wafers called "4NITDAN" and one for 6" wafers called "6NITDAN". The old LPCVD nitride furnace is mainly dedicated for deposition of low stress nitride, which does affect the cleanliness of the furnace, but stoichiometric nitride can also be deposited in the furnace. On this furnace the process for stoichiometric nitride is called "NITRIDE", and the process for low stress nitride (silicon rich nitride) is called "SIRICH"
Process parameters for the two standard deposition recipes on the old nitride furnace:
| Recipe name | Wafer size and number of wafers | Temperature [oC] | Pressure [mTorr] | NH3 gas flow [sccm] | DCS gas flow [sccm] | Comments |
|---|---|---|---|---|---|---|
| "NITRIDE" | 4" wafers
1-35 wafers in a run |
800 - 825 | 230 | 75 | 25 | Stoichiometric nitride |
| "SIRICH" | 4" wafers
1-35 wafers in a run |
835 | 112 | 13 | 93 | Low stress nitride (silicon rich nitride)
This was first tested at DTU Danchip by Matthias Heschel, |
Expected results when using the two standard recipes on the old nitride furnace:
These are typical values
| Recipe name | Deposition rate [Å/min] | Refractive index@630nm | Thickness variation on wafer | Thickness variation along the boat | Stress [MPa] |
|---|---|---|---|---|---|
| "NITRIDE" | 46-52 | 2.01-2.02 | <1.3% | <4% | 1000 |
| "SIRICH" | 30-40 | 2.20-2.30 | <5% | <20% | (-50 to 50) |
Process parameters for the two standard deposition recipes on the new nitride furnace:
| Recipe name | Wafer size and number of wafers | Temperature [oC] | Pressure [mTorr] | NH3 gas flow [sccm] | DCS gas flow [sccm] | Comments |
|---|---|---|---|---|---|---|
| "4NITDAN" | 4" wafers
1-25 wafers in a run |
780 - 790 | 200 | 100 | 33 | Stoichiometric nitride |
| "6NITDAN" | 6" wafers
1-25 wafers in a run |
780 - 790 | 200 | 120 | 30 | Stoichiometric nitride |
Expected results when using the two standard recipes on the new nitride furnace:
These are typical values
| Recipe name | Deposition rate [Å/min] | Refractive index@630nm | Thickness variation on wafer | Thickness variation along the boat | Stress [MPa] |
|---|---|---|---|---|---|
| "4NITDAN" | ~ 30-35 | 2.00 - 2.01 | <3% | <3% | |
| "6NITDAN" | ~ 30-35 | 2.00 - 2.01 | <3% |
Using LPCVD silicon nitride as a masking material for KOH etching
At Danchip stoichiometric silicon nitride is mainly used as masking material for potassium hydroxide (KOH) etching. The etch rate of the nitride in 80 oC KOH is expected to be less than 1 Å/min.
There are regularly users having problems with pinholes in the silicon nitride after KOH etching. It is not always clear what the reasons are, but we suspect problems can arise due to
- too many or too large particles in the nitride.
- too rough handling of the wafers after the nitride deposition.
- too much stress between the nitride and the underlying layer.
Our recommendations to try and avoid pinhole problems are:
To avoid too many or too large particles in the nitride<br\>
- Use the new nitride furnace, if you have to deposit stoichiometric nitride. In order to avoid problems with particles it is not allowed to deposit low stress nitride in this furnace, and the particles level is therefore low compared to the older nitride furnace
- Before running a process keep in close contact with the Danchip staff (especially the process specialist on the furnace) or take a look at the logbook to make sure that the nitride furnace is expected to be in a good state.
To avoid too rough handling of the wafers after the nitride deposition<br\>
- After the deposition handle the wafers with a clean glove on the edge of the wafers (no tweezers).
- Be careful not to scratch wafers with nitride (e.g. up against each other or on the spinner or the aligner).
- If you have nitride on the back side of a wafer while aligning, consider if you can protect it with e.g. a photoresist layer before loading it onto the aligner. Or use a non-vacuum aligner chuck with a big hole in the middle, so that the wafer is only laying on the edge. Avoid hard contact in the aligner if possible.
To avoid too much stress between the nitride and the underlying layer<br\>
- It is recommended to have a of silicon oxide layer between the silicon substrate and the nitride layer to reduce the stress level between the layers. The silicon nitride is then expected to have less tendency to break.
for sjov

Failed to parse (unknown function "\includegraphics"): {\displaystyle \includegraphics[width=0.5\textwidth]{RIE1_Si_Angle_O2_CHF3.jpg} \caption{The simplified model, which can be used in stead of the one in figure. In this representation is the total resistance in the entire transmission lines, not just between the capacitors.} }