At the moment DANCHIP has 3 PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
Recipes on PECVD1 for deposition of silicon oxides
Recipes
| Recipe name | SiH4 flow [sccm] | NO flow [sccm] | N2 flow [sccm] | B2H6 flow [sccm] | PH3 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| 1oxide/standard | 17 | 1600 | 0 | 0 | 0 | 400 | 380LF | Developed for waveguides |
| 1PBSG | Developed for waveguide top cladding by Haiyan Ou @DTU Photonics |
Expected results
| Recipe name | Deposition rate [µm/min] | RI | Uniformity [%] |
| 1oxide/standard | ~0.193 | 1.46 | 2 |
| 1PBSG | ~0.3 |
Recipes on PECVD2 for deposition of silicon oxides
Recipes
| Recipe name | SiH4 flow [sccm] | NO flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| 1STOxide | 12 | 1420 (setting in software is 710) | 392 | 550 | 100 |
LF=Low Frequency
Expected results
| Recipe name | Deposition rate [nm/min] | RI | Uniformity [%] |
| LFSiO | ~100 | ~1.47 | <1 |
Recipes on PECVD3 for deposition of silicon oxides
Recipes
| Recipe name | SiH4 flow [sccm] | NO flow [sccm] | N2 flow [sccm] | Pressure [mTorr] | Power [W] | Description |
| LFSiO | 12 | 1420 | 392 | 550 | 60 |
LF=Low Frequency
Expected results
| Recipe name | Deposition rate [nm/min] | RI | Uniformity [%] |
| LFSiO | ~81 | ~1.48 | <1 |