Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system: Difference between revisions
| Line 434: | Line 434: | ||
image:Kaempe_Lesker_standard_recipe_name.png| Deposition rate of HfO<sub>2</sub> at 150 <sup>o</sup>C. Substrate: Silicon 6" wafer with native oxide. | image:Kaempe_Lesker_standard_recipe_name.png| Deposition rate of HfO<sub>2</sub> at 150 <sup>o</sup>C. Substrate: Silicon 6" wafer with native oxide. | ||
</gallery> | </gallery> | ||
{| border="2" cellspacing="0" cellpadding="9" | |||
!colspan="1" border="none" style="background:silver; color:black;" align="center"|Recipe name | |||
|style="background:silver; color:black"|<b>Target material</b> | |||
|style="background:silver; color:black"|<b>Pressure (mTorr)</b> | |||
|style="background:silver; color:black"|<b>Power (W)</b> | |||
|style="background:silver; color:black"|<b>Deposition rate (nm/min)</b> | |||
|style="background:silver; color:black"|<b>Uniformity (%)<br> on 6 inch wafer</b> | |||
|style="background:silver; color:black"|<b>Comments</b> | |||
|- | |||
!style="background:silver; color:black;" align="center" |MD PC1 Src1 RF Upstream | |||
|style="background:LightGrey; color:black" align="center"|<b>SiO<sub>2</sub></b> | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"|140 (RF) | |||
|style="background:WhiteSmoke; color:black" align="center"|2.3 | |||
|style="background:WhiteSmoke; color:black" align="center"|0.5 | |||
|style="background:WhiteSmoke; color:black" align="center"| | |||
|- | |||
!style="background:silver; color:black;" align="center" |MD PC1 Src2 RF Upstream | |||
|style="background:LightGrey; color:black" align="center"|<b>SiO<sub>2</sub></b> | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"|140 (RF) | |||
|style="background:WhiteSmoke; color:black" align="center"|2.6 | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"| | |||
|- | |||
!style="background:silver; color:black;" align="center" |MD PC1 Src3 DC Upstream | |||
|style="background:LightGrey; color:black" align="center"|<b>Ni</b> | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"|500 (DC) | |||
|style="background:WhiteSmoke; color:black" align="center"|23.3 | |||
|style="background:WhiteSmoke; color:black" align="center"|2.5 | |||
|style="background:WhiteSmoke; color:black" align="center"| | |||
|- | |||
!style="background:silver; color:black;" align="center" |MD PC1 Src4 DC Upstream | |||
|style="background:LightGrey; color:black" align="center"|<b>Cu</b> | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"|500 (DC) | |||
|style="background:WhiteSmoke; color:black" align="center"|52.2 | |||
|style="background:WhiteSmoke; color:black" align="center"|2.2 | |||
|style="background:WhiteSmoke; color:black" align="center"| | |||
|- | |||
!style="background:silver; color:black;" align="center" |MD PC1 Src5 DC Upstream | |||
|style="background:LightGrey; color:black" align="center"|<b>Al</b> | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"|200 (DC) | |||
|style="background:WhiteSmoke; color:black" align="center"|7.9 | |||
|style="background:WhiteSmoke; color:black" align="center"|3.2 | |||
|style="background:WhiteSmoke; color:black" align="center"| | |||
|- | |||
!style="background:silver; color:black;" align="center" |MD PC1 Src5 Pulse DC<br> Downstream with reactive O<sub>2</sub> | |||
|style="background:LightGrey; color:black" align="center"|<b>Cu</b> | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"|500 (PDC)<br><b>Frequency:</b>100Hz<br><b>Reverse time:</b> 2µs | |||
|style="background:WhiteSmoke; color:black" align="center"|1.7 | |||
|style="background:WhiteSmoke; color:black" align="center"|3.4 | |||
|style="background:WhiteSmoke; color:black" align="center"|<b>Ar flow:</b>50sccm<br><b>O<sub>2</sub> flow:</b> 15 sccm | |||
|- | |||
!style="background:silver; color:black;" align="center" |MD PC1 Src6 Pulse DC Upstream | |||
|style="background:LightGrey; color:black" align="center"|<b>ITO</b> | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"|140 (PDC)<br><b>Frequency:</b>100Hz<br><b>Reverse time:</b> 2µs | |||
|style="background:WhiteSmoke; color:black" align="center"|11 | |||
|style="background:WhiteSmoke; color:black" align="center"|4.5 | |||
|style="background:WhiteSmoke; color:black" align="center"| | |||
|- | |||
!style="background:silver; color:black;" align="center" |MD PC1 Src6 Pulse DC<br> Downstream with reactive O<sub>2</sub> | |||
|style="background:LightGrey; color:black" align="center"|<b>ITO</b> | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"|140 (PDC)<br><b>Frequency:</b>100Hz<br><b>Reverse time:</b> 2µs | |||
|style="background:WhiteSmoke; color:black" align="center"|11.3 | |||
|style="background:WhiteSmoke; color:black" align="center"|- | |||
|style="background:WhiteSmoke; color:black" align="center"|<b>Ar flow:</b>50sccm<br><b>O<sub>2</sub> flow:</b> 2 sccm | |||
|- | |||
!style="background:silver; color:black;" align="center" |MD PC1 Src1 RF Upstream | |||
|style="background:LightGrey; color:black" align="center"|<b>Si</b> | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"|120 (RF) | |||
|style="background:WhiteSmoke; color:black" align="center"|1.8 | |||
|style="background:WhiteSmoke; color:black" align="center"|- | |||
|style="background:WhiteSmoke; color:black" align="center"| | |||
|- | |||
!style="background:silver; color:black;" align="center" |MD PC3 Src1 Pulse DC<br> Downstream with reactive N<sub>2</sub> | |||
|style="background:LightGrey; color:black" align="center"|<b>Al</b> | |||
|style="background:WhiteSmoke; color:black" align="center"|3 | |||
|style="background:WhiteSmoke; color:black" align="center"|900 (PDC)<br><b>Frequency:</b>100Hz<br><b>Reverse time:</b> 2µs | |||
|style="background:WhiteSmoke; color:black" align="center"|29 | |||
|style="background:WhiteSmoke; color:black" align="center"|3.2 | |||
|style="background:WhiteSmoke; color:black" align="center"|<b>Ar flow:</b>50sccm<br><b>O<sub>2</sub> flow:</b> 15 sccm | |||
|- | |||
|} | |||
Revision as of 22:27, 21 March 2020
Feedback to this page: click here

Cluster-based multi-chamber high vacuum sputtering deposition system is a robotic cluster tool with two deposition chambers sharing the same distribution trasfer station and the load-lock. The equipment has been installed and accepted in clean-room during January 2020. The purpose of the tool is to deposite variety of materials using DC/RF/PulseDC/HIPIMS magnetron sputtering with or without RF substrate bias. In modul A or PC 1 (process chamber 1) it is possible to deposit any materials using 6 x 3” magnetrons sourses with N2 or O2 reactive gases. Modul B or PC 3 (process chamber 3) is dedicated to oxygen free materials - nitrides and metals. It is eqipted with 1 x 4” + 2 x 3” magnetrons and supplied with N2 process gas for reactive deposition. Both chambers allow heating of substrates up to 600 oC. The equipment is located in clean-room A-5 where the user can acces the cassete loader.
Manufacture: Kurt J. Lesker Company
Model: 2017 PRO Line PVD75 thin film deposition cluster system
The user manual, user APV and contact information can be found in LabManager:
Sputter-System Metal-Oxide(PC1)
Sputter-System Metal-Nitride(PC3)
Thin Film group thinfilm@nanolab.dtu.dk is responsible of the equipment
Target/Metal requests should be sent to metal@nanolab.dtu.dk
If you need a training on the machine please send your request to: training@nanolab.dtu.dk.
Sputtering deposition system design
In the graphs below the HfO2 thickness vs. number of cycles for deposition temperatures between 150 oC and 350 oC presented. Results have been obtained for <100> 150 mm Si wafers with native oxide, based on ellipsometry study.
- Deposition rates of HfO2 at different temperaturs. ALD window.
-
Deposition rate of HfO2 at 150 oC. Substrate: Silicon 6" wafer with native oxide.
Power suppliy configuration
bla bla
| Power Supply ID | Type | Maximum output power (W) | Maximum output voltage (V) | Maximum output current (A) | Comments
|
|---|---|---|---|---|---|
| PC1 Power Supply 1 | RF | 300 | |||
| PC1 Power Supply 3 | DC | 500 | 1000 | 4 | |
| PC1 Power Supply 4 | DC | 500 | 1000 | 4 | |
| PC1 Power Supply 5 | Pulse DC | 2000 | 800 | 5 |
Max frequency: 100kHz |
| PC1 Power Supply 7 | RF (Substrate) | 100 | |||
| PC3 Power Supply 1 | RF | 300 | |||
| PC3 Power Supply 2 | Pulse DC | 2000 | 800 | 5 |
Max frequency: 100kHz |
| PC3 Power Supply 3 | DC to HiPIMS | 1500 | 1000 | 4 |
HiPIMS Unit
|
| PC3 Power Supply 5 | DC | 500 | 1000 | 4 |
|
| PC3 Power Supply 6 | RF (substrate) | 100 |
Sputter-System Metal-Oxide(PC1)
Bla bla
- Deposition rates of HfO2 at different temperaturs. ALD window.
-
Deposition rate of HfO2 at 150 oC. Substrate: Silicon 6" wafer with native oxide.
-
Deposition rate of HfO2 at 150 oC. Substrate: Silicon 6" wafer with native oxide.
Sputter-System Metal-Nitride(PC3)
bla bla
Bla bla
- Deposition rates of HfO2 at different temperaturs. ALD window.
-
Deposition rate of HfO2 at 150 oC. Substrate: Silicon 6" wafer with native oxide.
-
Deposition rate of HfO2 at 150 oC. Substrate: Silicon 6" wafer with native oxide.
Distribution Chamber (Genmark robot)
bla bla
- Deposition rates of HfO2 at different temperaturs. ALD window.
-
Deposition rate of HfO2 at 150 oC. Substrate: Silicon 6" wafer with native oxide.
Load lock
bla bla bla bla
Bla bla
- Deposition rates of HfO2 at different temperaturs. ALD window.
-
Deposition rate of HfO2 at 150 oC. Substrate: Silicon 6" wafer with native oxide.
-
Deposition rate of HfO2 at 150 oC. Substrate: Silicon 6" wafer with native oxide.
Process information
| Target size | Target material | Maximum Power density (W/inch2) | Maximum Power (W) | Maximum Ramp up/down Power (W/s) | Comments
|
|---|---|---|---|---|---|
| 3 inch | Al | 150 | 1000 | 10 | DC/HiPIMS |
| Au | 100 | 700 | 10 | DC/HiPIMS | |
| Ag | 100 | 700 | 10 | DC/HiPIMS | |
| Cu | 200 | 1400 | 10 | DC/HiPIMS | |
| Ni | 50 | 350 | 10 | High strengh magnets/DC | |
| Ti | 50 | 350 | 10 | DC/HiPIMS | |
| Ge (Bonded) | 20 | 140 | 0.3 | DC/RF | |
| Si (Unbonded/Bonded) | 20 | 140 | 0.3 | RF
| |
| SiO2 (Bonded) | 20 | 140 | 0.3 | RF
| |
| ITO (Bonded) | 20 | 140 | 0.3 | RF/PDC
| |
| BaTiO3 (Bonded) | 20 | 140 | 0.3 | RF
| |
| NbTi | 50 | 350 | 10 | DC | |
| 4 inch | Al | 150 | 1800 | 10 | DC/HiPIMS |
There are in total 76 developed and tested process recipes for general users (48 for PC1 and 28 for PC3). Starting the recipe the user can change te relevant process parameters: power, pressure, reactive gas ratio, rotation speed, substrate bias etc. In addition to the process recipes, there are also recipes for substrate heating and RF cleaning.
Bla bla
- Deposition rates of HfO2 at different temperaturs. ALD window.
-
Deposition rate of HfO2 at 150 oC. Substrate: Silicon 6" wafer with native oxide.
| Recipe name | Target material | Pressure (mTorr) | Power (W) | Deposition rate (nm/min) | Uniformity (%) on 6 inch wafer |
Comments
|
|---|---|---|---|---|---|---|
| MD PC1 Src1 RF Upstream | SiO2 | 3 | 140 (RF) | 2.3 | 0.5 | |
| MD PC1 Src2 RF Upstream | SiO2 | 3 | 140 (RF) | 2.6 | 3 | |
| MD PC1 Src3 DC Upstream | Ni | 3 | 500 (DC) | 23.3 | 2.5 | |
| MD PC1 Src4 DC Upstream | Cu | 3 | 500 (DC) | 52.2 | 2.2 | |
| MD PC1 Src5 DC Upstream | Al | 3 | 200 (DC) | 7.9 | 3.2 | |
| MD PC1 Src5 Pulse DC Downstream with reactive O2 |
Cu | 3 | 500 (PDC) Frequency:100Hz Reverse time: 2µs |
1.7 | 3.4 | Ar flow:50sccm O2 flow: 15 sccm
|
| MD PC1 Src6 Pulse DC Upstream | ITO | 3 | 140 (PDC) Frequency:100Hz Reverse time: 2µs |
11 | 4.5 | |
| MD PC1 Src6 Pulse DC Downstream with reactive O2 |
ITO | 3 | 140 (PDC) Frequency:100Hz Reverse time: 2µs |
11.3 | - | Ar flow:50sccm O2 flow: 2 sccm |
| MD PC1 Src1 RF Upstream | Si | 3 | 120 (RF) | 1.8 | - | |
| MD PC3 Src1 Pulse DC Downstream with reactive N2 |
Al | 3 | 900 (PDC) Frequency:100Hz Reverse time: 2µs |
29 | 3.2 | Ar flow:50sccm O2 flow: 15 sccm |