Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using PECVD: Difference between revisions

Bghe (talk | contribs)
No edit summary
Bghe (talk | contribs)
 
(8 intermediate revisions by the same user not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_Silicon_Oxide_using_PECVD  click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_Silicon_Oxide_using_PECVD  click here]'''<br>
{{CC-bghe1}}


''This page is written by Berit Herstrøm @ DTU Nanolab is nothing else is stated''<br>


At the moment DTU Nanolab has 2 PECVDs that can deposit silicon oxide with or without dopants of boron, phosphorus. PECVD1 and PECVD2 has been decommissioned and now we have PECVD3 and PECVD4. PECVD3 are for silicon based processing allowing wafers with small amount of metal (<5% wafer coverage). PECVD4 is for clean wafers both for silicon based materials and for III-V materials. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at Nanolab. All though PECVD4 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system.
At the moment DTU Nanolab has 2 PECVDs that can deposit silicon oxide with or without dopants of boron, phosphorus. PECVD1 and PECVD2 has been decommissioned and now we have PECVD3 and PECVD4. PECVD3 are for silicon based processing allowing wafers with small amount of metal (<5% wafer coverage). PECVD4 is for clean wafers both for silicon based materials and for III-V materials. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at Nanolab. All though PECVD4 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system.
Line 10: Line 10:
|-
|-
|
|
*[http://labmanager.dtu.dk/d4Show.php?id=5093&mach=395 The QC procedure for PECVD4]<br>
*[http://labmanager.dtu.dk/d4Show.php?id=5093&mach=395 The QC procedure for PECVD4 - requires login]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=395 The newest QC data for PECVD4]
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=395 The newest QC data for PECVD4 - requires login]
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
Line 39: Line 39:
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
!QC limits
!QC limits
!PECVD3 - OXIDE
!PECVD4 - OXIDE
|-
|-
|Deposition rate
|Deposition rate
Line 180: Line 180:
|-
|-
|
|
*[http://labmanager.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3]<br>
*[http://labmanager.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3 - requires login]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3]
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3 - requires login]
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
Line 278: Line 278:
|Uniformity [%]
|Uniformity [%]
|Stress
|Stress
|Comment
|-
|-
|LFSiO2
|LFSiO2
Line 284: Line 285:
|~1.5%
|~1.5%
|'''400-402 MPa''' compressive stress '' by Anders Simonsen @nbi.ku.dk April 2016''
|'''400-402 MPa''' compressive stress '' by Anders Simonsen @nbi.ku.dk April 2016''
|We have seen that this recipe does not deposit the first minute
|-  
|-  
|LFSiO
|LFSiO
Line 290: Line 292:
|<1
|<1
|not measured
|not measured
|.
|-
|-
|1PBSG
|1PBSG
Line 296: Line 299:
|~17%
|~17%
|not measured
|not measured
|.
|}
|}
<br clear="all" />
<br clear="all" />
Line 314: Line 318:
|Description
|Description
|-  
|-  
|Core-Ge
|Core-Ge (not possible anymore as we have no Germanium)
|17
|17
|1600
|1600
Line 354: Line 358:
|~1.458  
|~1.458  
|}
|}


=Recipes on PECVD2 for deposition of silicon oxides <span style="color:Red">EXPIRED!!!</span>=
=Recipes on PECVD2 for deposition of silicon oxides <span style="color:Red">EXPIRED!!!</span>=
Line 363: Line 366:
|-
|-
|
|
*[http://labmanager.dtu.dk/d4Show.php?id=1988&mach=17 The QC procedure for PECVD2]<br>
 
*[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=17 The newest QC data for PECVD2]
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |