Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Chromium/Thermal evaporation of Cr in Thermal evaporator: Difference between revisions

Eves (talk | contribs)
Created page with "== '''Thermal evaporation of Chromium''' == Chromium can be thermally evaporated in the Thermal Evaporator (NANO 36 THERMAL EVAPORATOR SYSTEM). At DTU Nanolab, we use dedicat..."
 
Reet (talk | contribs)
No edit summary
 
(62 intermediate revisions by 3 users not shown)
Line 1: Line 1:
== '''Thermal evaporation of Chromium''' ==
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Chromium/Thermal_evaporation_of_Cr_in_Thermal_evaporator click here]'''
 
 
<i>This page is written by <b>Evgeniy Shkondin @DTU Nanolab</b> if nothing else is stated. <br>
All images and photos on this page belongs to <b>DTU Nanolab</b>.<br>
The fabrication and characterization described below were conducted in <b>2020 by Evgeniy Shkondin.</b> The shield design was developed by <b>Henrik Nielsen (Nanolab, ThinFilm)</b>, and built by Nanolab Facility service</b>.<br></i>
 
 
= Thermal evaporation of Chromium=
 
Chromium can be thermally evaporated in the [[Specific_Process_Knowledge/Thin_film_deposition/thermalevaporator|Thermal Evaporator]] (NANO 36 THERMAL EVAPORATOR SYSTEM). At DTU Nanolab, for the Cr thermal source we have experimented with Cr pellets in a W boat as well as dedicated 4" long chromium plated tungsten rods (supplier: KJLC).
 
The process and resulting material characteristics described on this page were done using the Cr plated W rod. However, we have found that using Cr pellets is easier in the long run as it does not require modifying the chamber layout. So the current method you will most likely use is evaporation of Cr pellets from a boat (2025). There will be some differences from what is described below, e.g., uniformity will be different. You can still use the results from XRD/XRR, XPS, SEM, and AFM as an indication of what you might expect and as a guide for relevant investigations.
 
==Cr evaporation from Cr-coated W rod==
 
During power ramp up, the material warms up and sublimates. Unlike deposition of Al and Ag, where simple crucibles are used with point-source evaporation from bottom to the substrate, the deposition of chromium from a coated rod proceeds in all directions. To prevent the deposition on the side-walls and the bottom of the chamber a specific protecting shield is mounted beneath the tungsten rod.
 
<b>The shield design was developed by Henrik Nielsen (Nanolab, ThinFilm), and build by Nanolab Facility service. The process was developed and tested by Evgeniy Shkondin (Nanolab, ThinFilm) in december 2020.</b>


Chromium can be thermally evaporated in the Thermal Evaporator (NANO 36 THERMAL EVAPORATOR SYSTEM). At DTU Nanolab, we use dedicated 4" long chrome plated tungsten rods (supplier: KJLC). During power ramp up, the material warms up and sublimates. Unlike deposition of Al and Ag, where simple crucibles are used with point-source evaporation from bottom to the substrate, the Deposition of chromium proceeds in all directions. To prevent the deposition on the side-walls and the bottom of the chamber a specific protecting shield is mounted beneath the tungsten rod.


<gallery caption="" widths="600px" heights="400px" perrow="2">
<gallery caption="" widths="600px" heights="400px" perrow="2">
Line 8: Line 25:
</gallery>
</gallery>


== '''Set-up installation''' ==
== '''Set-up and installation of the rod''' ==
 
The deposition of Chromium requires a major change of the tool hardware installation. Ask Nanolab responsible employee if you need to perform this change.


<gallery caption="" widths="600px" heights="400px" perrow="3">
<gallery caption="" widths="600px" heights="400px" perrow="3">
Line 18: Line 37:
</gallery>
</gallery>


== '''Recipe''' ==
== '''Recipe and process performance''' ==
 
The photographs illustrate recipe parameters.


<gallery caption="" widths="800px" heights="800px" perrow="1">
image:eves_Cr_thermal_evaporation_recipe.png|Figure 8. Different windows of the recipe controller.
</gallery>
== '''Process development''' ==
=== '''Initial test runs''' ===
=== '''First run''' ===
The initial tooling factor is 148%. 6" wafer is loaded with a shadowed mask. Measured base pressure before start is in order of 10<sup>-7</sup> Torr, since the chamber stayed pumped for a few hours. Deposition thickness setpoint is set to 100 nm.


{| border="2" cellspacing="0" cellpadding="9"  
{| border="2" cellspacing="0" cellpadding="9"  


 
!colspan="1" border="none" style="background:WhiteSmoke; color:black;" align="center"|Deposition rate (Å/s)  
!colspan="1" border="none" style="background:silver; color:black;" align="center"|Pressure (Torr)
|style="background:WhiteSmoke; color:black"|<b>1</b>*
|style="background:silver; color:black"|<b>Deposition rate (Å/s)</b>
|style="background:silver; color:black"|<b>Output power (W)</b>
|style="background:silver; color:black"|<b>Deposited thickness (nm)</b>
|style="background:silver; color:black"|<b>Comment</b>
 
|-
!style="background:WhiteSmoke; color:black;" align="center"|-
 
|style="background:WhiteSmoke; color:black" align="center"|1.0
 
|style="background:WhiteSmoke; color:black" align="center"|24.4
 
|style="background:WhiteSmoke; color:black" align="center"|0
 
|style="background:WhiteSmoke; color:black" align="center"|-
 
|-
!style="background:WhiteSmoke; color:black" align="center"|1.1 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|1.0
 
|style="background:WhiteSmoke; color:black" align="center"|25.1
 
|style="background:WhiteSmoke; color:black" align="center"|10
 
|style="background:WhiteSmoke; color:black" align="center"|-
 
|-
!style="background:WhiteSmoke; color:black" align="center"|1.1 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|1.0
 
|style="background:WhiteSmoke; color:black" align="center"|27
 
|style="background:WhiteSmoke; color:black" align="center"|20
 
|style="background:WhiteSmoke; color:black" align="center"|Cr started to retract from one of the sides toward another (30% opened area)
 
|-
!style="background:WhiteSmoke; color:black" align="center"|1.2 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.94
 
|style="background:WhiteSmoke; color:black" align="center"|28.7
 
|style="background:WhiteSmoke; color:black" align="center"|30
 
|style="background:WhiteSmoke; color:black" align="center"|(40% opened area)
 
|-
!style="background:WhiteSmoke; color:black" align="center"|1.3 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.94
 
|style="background:WhiteSmoke; color:black" align="center"|30.4
 
|style="background:WhiteSmoke; color:black" align="center"|40
 
|style="background:WhiteSmoke; color:black" align="center"|(45% opened area)


|-
|-
!style="background:WhiteSmoke; color:black" align="center"|1.4 10<sup>-7</sup>
!style="background:WhiteSmoke; color:black;" align="center"|Maximum Thickness
 
|style="background:WhiteSmoke; color:black" align="center"|<b>100 nm</b>**
|style="background:WhiteSmoke; color:black" align="center"|0.94
 
|style="background:WhiteSmoke; color:black" align="center"|32.1
 
|style="background:WhiteSmoke; color:black" align="center"|50
 
|style="background:WhiteSmoke; color:black" align="center"|(50% opened area)


|-
|-
!style="background:WhiteSmoke; color:black" align="center"|1.5 10<sup>-7</sup>
!style="background:WhiteSmoke; color:black" align="center"|Film Tooling
 
|style="background:WhiteSmoke; color:black" align="center"|<b>173 %</b>
|style="background:WhiteSmoke; color:black" align="center"|0.95
 
|style="background:WhiteSmoke; color:black" align="center"|34.1
 
|style="background:WhiteSmoke; color:black" align="center"|60
 
|style="background:WhiteSmoke; color:black" align="center"|(60% opened area)


|-
|-
!style="background:WhiteSmoke; color:black" align="center"|1.7 10<sup>-7</sup>
!style="background:WhiteSmoke; color:black" align="center"|Density
 
|style="background:WhiteSmoke; color:black" align="center"|<b>7.2 g/cm<sup>3</sup></b>
|style="background:WhiteSmoke; color:black" align="center"|0.92
 
|style="background:WhiteSmoke; color:black" align="center"|36.3
 
|style="background:WhiteSmoke; color:black" align="center"|70
 
|style="background:WhiteSmoke; color:black" align="center"|(65-70% opened area)
 
|-
!style="background:WhiteSmoke; color:black" align="center"|2.6 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.92
 
|style="background:WhiteSmoke; color:black" align="center"|38.7
 
|style="background:WhiteSmoke; color:black" align="center"|80
 
|style="background:WhiteSmoke; color:black" align="center"|(80% opened area)
 
|-
!style="background:WhiteSmoke; color:black" align="center" |5.4 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.91
 
|style="background:WhiteSmoke; color:black" align="center"|41.5
 
|style="background:WhiteSmoke; color:black" align="center"|90
 
|style="background:WhiteSmoke; color:black" align="center"|(90% opened area)


|-
|-
!style="background:WhiteSmoke; color:black" align="center" |8.7 10<sup>-7</sup>
!style="background:WhiteSmoke; color:black" align="center"|Z-factor
 
|style="background:WhiteSmoke; color:black" align="center"|<b>0.305</b>
|style="background:WhiteSmoke; color:black" align="center"|0.92
 
|style="background:WhiteSmoke; color:black" align="center"|43.9
 
|style="background:WhiteSmoke; color:black" align="center"|100
 
|style="background:WhiteSmoke; color:black" align="center"|(96% opened area, almost all Cr is gone now and emptied W rod illuminates a very bright light.)


|-  
|-  
|}
|}


<br>
'''*''' The deposition rate can be increased (up to 2Å/s or even 5 Å/s), but it requires a new recipe.
<!-- -->


[[image:eves_20210126_Cr_thermal_evaporator_08.png|center|300x300px|thumb|Figure 9. Thickness distribution across 6" wafer.]]
'''**'''Although it is possible to deposit 100 nm, we do not recommend exceeding the thickness setpoint above <b>80 nm</b>, due to instabilities at the end.


<br>
<br>
<!-- -->
<!-- -->


=== '''Second run''' ===
=== '''Deposition of 100 nm''' ===
The adjusted tooling factor is 173%. 6" wafer is loaded with a shadowed mask. Measured base pressure before start 7 10<sup>-6</sup> Torr. Deposition thickness setpoint is set to 100 nm.
 
{| border="2" cellspacing="0" cellpadding="9"


The adjusted tooling factor 173%. Full 6" wafer is loaded with shadow-mask. No rotation. Deposition thickness setpoint is set to 100 nm.


!colspan="1" border="none" style="background:silver; color:black;" align="center"|Pressure (Torr)
Pressure fluctuations during the ramp-up:
|style="background:silver; color:black"|<b>Deposition rate (Å/s)</b>
|style="background:silver; color:black"|<b>Output power (W)</b>
|style="background:silver; color:black"|<b>Deposited thickness (nm)</b>
|style="background:silver; color:black"|<b>Comment</b>
 
|-
!style="background:WhiteSmoke; color:black;" align="center"|1.9 10<sup>-6</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|1.0
 
|style="background:WhiteSmoke; color:black" align="center"|24.3
 
|style="background:WhiteSmoke; color:black" align="center"|0
 
|style="background:WhiteSmoke; color:black" align="center"|fine
 
|-
!style="background:WhiteSmoke; color:black" align="center"|7.9 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.97
 
|style="background:WhiteSmoke; color:black" align="center"|24.6
 
|style="background:WhiteSmoke; color:black" align="center"|10
 
|style="background:WhiteSmoke; color:black" align="center"|fine
 
|-
!style="background:WhiteSmoke; color:black" align="center"|5.9 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.97
 
|style="background:WhiteSmoke; color:black" align="center"|25.5
 
|style="background:WhiteSmoke; color:black" align="center"|20
 
|style="background:WhiteSmoke; color:black" align="center"|fine
 
|-
!style="background:WhiteSmoke; color:black" align="center"|5.7 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.97
 
|style="background:WhiteSmoke; color:black" align="center"|26.1
 
|style="background:WhiteSmoke; color:black" align="center"|30
 
|style="background:WhiteSmoke; color:black" align="center"|fine
 
|-
!style="background:WhiteSmoke; color:black" align="center"|6.1 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.98
 
|style="background:WhiteSmoke; color:black" align="center"|26.4
 
|style="background:WhiteSmoke; color:black" align="center"|40
 
|style="background:WhiteSmoke; color:black" align="center"|fine
 
|-
!style="background:WhiteSmoke; color:black" align="center"|6.6 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|1.0
 
|style="background:WhiteSmoke; color:black" align="center"|26.8
 
|style="background:WhiteSmoke; color:black" align="center"|56
 
|style="background:WhiteSmoke; color:black" align="center"|fine
 
|-
!style="background:WhiteSmoke; color:black" align="center"|6.9 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.99
 
|style="background:WhiteSmoke; color:black" align="center"|27.0
 
|style="background:WhiteSmoke; color:black" align="center"|60
 
|style="background:WhiteSmoke; color:black" align="center"|fine
 
|-
!style="background:WhiteSmoke; color:black" align="center"|7.4 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.99
 
|style="background:WhiteSmoke; color:black" align="center"|27.2
 
|style="background:WhiteSmoke; color:black" align="center"|70
 
|style="background:WhiteSmoke; color:black" align="center"|fine
 
|-
!style="background:WhiteSmoke; color:black" align="center"|7.6 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|0.99
 
|style="background:WhiteSmoke; color:black" align="center"|27.3
 
|style="background:WhiteSmoke; color:black" align="center"|80
 
|style="background:WhiteSmoke; color:black" align="center"|fine
 
|-
!style="background:WhiteSmoke; color:black" align="center" |7.9 10<sup>-7</sup>
 
|style="background:WhiteSmoke; color:black" align="center"|1.0
 
|style="background:WhiteSmoke; color:black" align="center"|27.4
 
|style="background:WhiteSmoke; color:black" align="center"|90
 
|style="background:WhiteSmoke; color:black" align="center"|fine
 
|-
!style="background:WhiteSmoke; color:black" align="center" |-
 
|style="background:WhiteSmoke; color:black" align="center"|-
 
|style="background:WhiteSmoke; color:black" align="center"|-
 
|style="background:WhiteSmoke; color:black" align="center"|100
 
|style="background:WhiteSmoke; color:black" align="center"|(Cr still intact all places on the rod, only at the centrum some slightly visible retraction.)
 
|-
|}
 
<br>
<!-- -->
 
[[image:eves_20210126_Cr_thermal_evaporator_09.png|center|300x300px|thumb|Figure 10. Thickness distribution across 6" wafer.]]
 
<br>
<!-- -->
 
=== '''Third run''' ===
 
The adjusted tooling factor 173% was fine. Full 6" wafer is loaded for film characterisation. Measured base pressure before start 4.4 10<sup>-6</sup> Torr. Waited 1 hour before start. Deposition thickness setpoint is set to 100 nm.
 
Pressure fluctuations:
* Rise 1 phase @ 0-15W: 4.4 10<sup>-6</sup> Torr &#8594; 6.2 10<sup>-6</sup> Torr
* Rise 1 phase @ 0-15W: 4.4 10<sup>-6</sup> Torr &#8594; 6.2 10<sup>-6</sup> Torr
* Soak 1 phase @ 15W: 6.2 10<sup>-6</sup> Torr &#8594; 10<sup>-5</sup> Torr &#8594; 6.5 10<sup>-6</sup> Torr
* Soak 1 phase @ 15W: 6.2 10<sup>-6</sup> Torr &#8594; 10<sup>-5</sup> Torr &#8594; 6.5 10<sup>-6</sup> Torr
Line 463: Line 214:
|-  
|-  
|}
|}
<br>
<!-- -->
[[image:eves_20210126_Cr_thermal_evaporator_09.png|center|300x300px|thumb|Figure 8. Thickness distribution across 6" wafer. Measurement is performed using [[Specific_Process_Knowledge/Characterization/Dektak_XTA|Dektak stylus profilometer]].]]


<br>
<br>
Line 470: Line 227:


<gallery caption="" widths="500px" heights="400px" perrow="1">
<gallery caption="" widths="500px" heights="400px" perrow="1">
image:eves_Cr_retraction.png|Figure 11. Cr retraction from the tingsten rod at the end of lifetime.  
image:eves_Cr_retraction.png|Figure 9. Cr retraction from the tingsten rod at the end of lifetime.  
</gallery>
</gallery>
The limited amount of chromium, the nature of deposition (in all directions) and retruction sets a limit on how thick layer can be deposited. We do not recomend to exeed the thickness above 80 nm, and do not allow thicknesses above 100 nm.
Note! <b>Remember to discard the used tungsten rods. Never reinstall them. Always mount a new source.</b>


== '''Film characterisation''' ==
== '''Film characterisation''' ==
Full 6" wafer is loaded for film characterization. Measured base pressure before start 4.4 10-6 Torr. Waited 1 hour before start. Deposition thickness setpoint is set to 100 nm. The prepared sample was cleaved into small pieces for characterization.


===X-ray reflectivity method===
===X-ray reflectivity method===


XRR measurements for Cr film has been performed using Rigaku XRD SmartLab diffractometer.
XRR measurements for Cr film has been performed using [[Specific_Process_Knowledge/Characterization/XRD/XRD_SmartLab|Rigaku XRD SmartLab diffractometer]].




<gallery caption="" widths="1200px" heights="400px" perrow="1">
<gallery caption="" widths="1200px" heights="400px" perrow="1">
image:eves_XRR_thermal_evaporator_Cr.png|Figure 12. XRR scan. Substrate: Silicon 6" wafer with native oxide.
image:eves_XRR_thermal_evaporator_Cr.png|Figure 10. XRR scan. Substrate: Silicon 6" wafer with native oxide.
</gallery>
</gallery>


The following model is selected for XRR fitting: Native chromium oxide, bulk chromium layer, native silicon oxide, and the bulk silicon substrate.
The following model is selected for XRR fitting: Native chromium oxide, bulk chromium layer, native silicon oxide, and the bulk silicon substrate. Fitting results presented in the table.




Line 532: Line 296:
|-  
|-  
|}
|}
<br>
<!-- -->


===In-Plane X-ray diffraction===
===In-Plane X-ray diffraction===


In-Plane diffraction spectrum acquired with Rigaku XRD SmartLab diffractometer. Incident angle <math>\omega = 0.4</math><sup>o</sup> IS=0.1mm, RS1=RS2=open. Scan speed: 1<sup>o</sup>/min.
 
In-Plane diffraction spectrum acquired with [[Specific_Process_Knowledge/Characterization/XRD/XRD_SmartLab|Rigaku XRD SmartLab diffractometer]]. Incident angle <math>\omega = 0.4</math><sup>o</sup> IS=0.1mm, RS1=RS2=open. Scan speed: 1<sup>o</sup>/min.
 
The diffraction pattern reveal a polycrystalline film with a strong <111> orientation peak.
 
<gallery caption="" widths="600px" heights="400px" perrow="1">
<gallery caption="" widths="600px" heights="400px" perrow="1">
image:eves_Cr_InPlane_XRD.png|Figure 13. In-Plane XRD scan. Substrate: Silicon 6" wafer with native oxide.
image:eves_Cr_InPlane_XRD.png|Figure 11. In-Plane XRD scan. Substrate: Silicon 6" wafer with native oxide.
</gallery>
</gallery>


===X-ray photoelectron spectroscopy===
===X-ray photoelectron spectroscopy===


XPS profiles for Al films has been obtained using XPS K-Alpha equipment.
XPS profiles for Cr films has been obtained using [[Specific_Process_Knowledge/Characterization/XPS/K-Alpha|XPS K-Alpha equipment]].




<gallery caption="" widths="600px" heights="400px" perrow="2">
<gallery caption="" widths="600px" heights="400px" perrow="2">
image:eves_20210128_XPS_survey.png|Figure 14. Survey scan of Cr thin film after 580 s. Ar<sup>+</sup> sputtering. Substrate: Silicon 6" wafer with native oxide.
image:eves_20210128_XPS_survey.png|Figure 12. Survey scan of Cr thin film after 580 s. Ar<sup>+</sup> sputtering. Substrate: Silicon 6" wafer with native oxide.
image:eves_20210128_C1s.png|Figure 15. High resolution of <b>C 1s</b> signal. At the surface native airborne carbon can be observed, the signal disappears immediately after the ion beam is turned on. Substrate: Silicon 6" wafer with native oxide.
image:eves_20210128_C1s.png|Figure 13. High resolution of <b>C 1s</b> signal. At the surface native airborne carbon can be observed, the signal disappears immediately after the ion beam is turned on. Substrate: Silicon 6" wafer with native oxide.
image:eves_20210128_Cr2p.png|Figure 16. High resolution <b>Cr 2p</b> signal during the depth profiling. Ar<sup>+</sup> sputtering proceeds from 0 to 580 s, with 20 s. interval with mid-current and energy of 3000 eV. At the surface, the Cr peak is doubled due the bonding to oxygen and bonding to Cr. After the etching the peak responsible to oxygen bonding becomes neglible. Substrate: Silicon 6" wafer with native oxide.
image:eves_20210128_Cr2p.png|Figure 14. High resolution <b>Cr 2p</b> signal during the depth profiling. Ar<sup>+</sup> sputtering proceeds from 0 to 580 s, with 20 s. interval with mid-current and energy of 3000 eV. At the surface, the Cr peak is doubled due the bonding to oxygen and bonding to Cr. After the etching the peak responsible to oxygen bonding becomes neglible. Substrate: Silicon 6" wafer with native oxide.
image:eves_20210128_O1s.png|Figure 17. High resolution of <b>O 1s</b> signal. The signal is obviously strong at the beginning, since the top layer is composed of CrO<sub>x</sub>, but it never completely disapears, but it becomes saturated, which means that some level of oxygen is always present. Substrate: Silicon 6" wafer with native oxide.
image:eves_20210128_O1s.png|Figure 15. High resolution of <b>O 1s</b> signal. The signal is obviously strong at the beginning, since the top layer is composed of CrO<sub>x</sub>, but it never completely disapears, but it becomes saturated, which means that some level of oxygen is always present. Substrate: Silicon 6" wafer with native oxide.
image:eves_Cr_thermal_evaporation_XPS_depth_profile.png|Figure 18. XPS depth profile. The top surface is oxidized, but the oxygen signal lowers, once getting deeper. Nevertheless, it remains around 10 at.% in the bulk layer. The is a strange nitrogen lower signal. The reason is unknown. Substrate: Silicon 6" wafer with native oxide.
image:eves_Cr_thermal_evaporation_XPS_depth_profile.png|Figure 16. XPS depth profile. The top surface is oxidized, but the oxygen signal lowers, once getting deeper. Nevertheless, it remains around 10 at.% in the bulk layer. The is a strange nitrogen lower signal. The reason is unknown. Substrate: Silicon 6" wafer with native oxide.


</gallery>
</gallery>
Line 557: Line 329:




SEM and AFM measurements illustrate surface morphology and roughness.  
[[Specific_Process_Knowledge/Characterization/SEM:_Scanning_Electron_Microscopy|SEM]] and [[Specific_Process_Knowledge/Characterization/AFM:_Atomic_Force_Microscopy|AFM]] measurements illustrate surface morphology and roughness.  




<gallery caption="" widths="600px" heights="400px" perrow="2">
<gallery caption="" widths="600px" heights="400px" perrow="2">
image:eves_Cr_thermal_evap_SEM_20210215.png|Figure 18. SEM image. Substrate: Silicon 6" wafer with native oxide.
image:eves_Cr_thermal_evap_SEM_20210215.png|Figure 17. SEM image. Substrate: Silicon 6" wafer with native oxide.
image:eves_Cr_thermal_evap_AFM_20210215.png|Figure 19. AFM image. Substrate: Silicon 6" wafer with native oxide.
image:eves_Cr_thermal_evap_AFM_20210215.png|Figure 18. AFM image. Substrate: Silicon 6" wafer with native oxide.