'''Feedback to this page''': '''[mailto:labadviser@ | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_Silicon_Oxide_using_PECVD click here]'''<br> | ||
{{CC-bghe1}} | |||
At the moment | At the moment DTU Nanolab has 2 PECVDs that can deposit silicon oxide with or without dopants of boron, phosphorus. PECVD1 and PECVD2 has been decommissioned and now we have PECVD3 and PECVD4. PECVD3 are for silicon based processing allowing wafers with small amount of metal (<5% wafer coverage). PECVD4 is for clean wafers both for silicon based materials and for III-V materials. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at Nanolab. All though PECVD4 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system. | ||
== Deposition of SiO2 with PECVD4 [[ | == Deposition of SiO2 with PECVD4 == | ||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD4 - oxide ''' | |||
|- | |||
| | |||
*[http://labmanager.dtu.dk/d4Show.php?id=5093&mach=395 The QC procedure for PECVD4 - requires login]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=395 The newest QC data for PECVD4 - requires login] | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:200px" | |||
! QC Recipe: | |||
! QCOXYD2 | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|12 sccm | |||
|- | |||
|N<sub>2</sub>O flow | |||
|1420 sccm | |||
|- | |||
|N<sub>2</sub> flow | |||
|392 sccm | |||
|- | |||
|Pressure | |||
|550 mTorr | |||
|- | |||
|RF-power | |||
|60 W | |||
|- | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
!QC limits | |||
!PECVD4 - OXIDE | |||
|- | |||
|Deposition rate | |||
|70 - 85 nm/min | |||
|- | |||
|Non-uniformity | |||
|<3.0 | |||
|- | |||
|Refractive index | |||
|1.474 - 1.486 | |||
|- | |||
|} | |||
|- | |||
|} | |||
|} | |||
{| border="1" cellspacing="2" cellpadding="2" | {| border="1" cellspacing="2" cellpadding="2" | ||
| Line 15: | Line 64: | ||
!|Comments | !|Comments | ||
!|SiH4 [sccm] | !|SiH4 [sccm] | ||
!|N2O [sccm] | !|N2O [sccm] | ||
!|N2 [sccm] | !|N2 [sccm] | ||
!|B2H6 | |||
!|PH3 | |||
!|Pressure [mTorr] | !|Pressure [mTorr] | ||
!|Power [W] | !|Power [W] | ||
| Line 27: | Line 77: | ||
|- | |- | ||
| | |LF SiO<!-- Recipe --> | ||
| | |75-78 nm/min<!-- Dep. rate [nm/min] --> | ||
| | |1.480-1.483<!-- RI --> | ||
|± 1.7%<!-- Unif. [%] --> | |± 2.1-2.7%<!-- Unif. [%] --> | ||
| | |compressive 309 MPa <!-- Stress [MPa] --> | ||
|<!-- Comments --> | |[[/LF_SiO2 results|Click for more results]]<!-- Comments --> | ||
| | |12<!-- SiH4 [sccm] --> | ||
| | |1420<!-- N2O [sccm] --> | ||
|<!-- N2O [sccm] --> | |392<!-- N2 [sccm] --> | ||
| | |<!-- B2H6 --> | ||
|<!-- PH3 --> | |||
|550 mTorr<!-- Pressure [mTorr] --> | |||
|60LF"<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|1:15/13:00(stress)<!-- Time [mm:ss] --> | |||
|February 2017 bghe<!--Tested --> | |||
|- | |||
|HF SiO<!-- Recipe --> | |||
|63-64 nm/min<!-- Dep. rate [nm/min] --> | |||
|1.476-1.477<!-- RI --> | |||
|± 0.3-0.5%<!-- Unif. [%] --> | |||
|Compressive: 250.5 MPa<!-- Stress [MPa] --> | |||
|[[/HF_SiO2 results|Click for more results]]<!-- Comments --> | |||
|10<!-- SiH4 [sccm] --> | |||
|1420<!-- N2O [sccm] --> | |||
|392<!-- N2 [sccm] --> | |||
|<!-- B2H6 --> | |||
|<!-- PH3 --> | |||
|900 mTorr<!-- Pressure [mTorr] --> | |900 mTorr<!-- Pressure [mTorr] --> | ||
| | |30HF<!-- Power [W] --> | ||
|<!-- Load --> | |<!-- Load --> | ||
|<!-- Tune --> | |<!-- Tune --> | ||
| | |2:00/16:00(stress)<!-- Time [mm:ss] --> | ||
|February 2017 bghe<!--Tested --> | |February 2017 bghe<!--Tested --> | ||
|- | |- | ||
| | |waveguide <!-- Recipe --> | ||
| | |159.5 nm/min<!-- Dep. rate [nm/min] --> | ||
|1. | |1.462<!-- RI --> | ||
|± | |± 0.8%<!-- Unif. [%] --> | ||
|Compressive: | |Compressive: 121.9 MPa<!-- Stress [MPa] --> | ||
|<!-- Comments --> | |<!-- Comments --> | ||
| | |17<!-- SiH4 [sccm] --> | ||
| | |2000<!-- N2O [sccm] --> | ||
|<!-- | |<!-- N2 [sccm] --> | ||
| | |<!-- B2H6 --> | ||
| | |<!-- PH3 --> | ||
| | |300 mTorr<!-- Pressure [mTorr] --> | ||
|700 LF<!-- Power [W] --> | |||
|<!-- Load --> | |<!-- Load --> | ||
|<!-- Tune --> | |<!-- Tune --> | ||
| | |40:00<!-- Time [mm:ss] --> | ||
|February 2017 bghe<!--Tested --> | |February 2017 bghe<!--Tested --> | ||
|- | |- | ||
| | |BPSG<!-- Recipe --> | ||
| | |259 nm/min<!-- Dep. rate [nm/min] --> | ||
| | |1.4593<!-- RI --> | ||
|± 1. | |± 1.7%<!-- Unif. [%] --> | ||
| | |Compressive: 36.7 MPa<!-- Stress [MPa] --> | ||
|<!-- Comments --> | |Measured after anneal in Clad1000<!-- Comments --> | ||
| | |17<!-- SiH4 [sccm] --> | ||
| | |1600<!-- N2O [sccm] --> | ||
|<!-- | |<!-- N2 [sccm] --> | ||
| | |135<!-- B2H6 --> | ||
|40<!-- PH3 --> | |||
|900 mTorr<!-- Pressure [mTorr] --> | |900 mTorr<!-- Pressure [mTorr] --> | ||
| | |800 LF <!-- Power [W] --> | ||
|<!-- Load --> | |<!-- Load --> | ||
|<!-- Tune --> | |<!-- Tune --> | ||
|10:00/56:00(stress)<!-- Time [mm:ss] --> | |10:00/56:00(stress)<!-- Time [mm:ss] --> | ||
|February 2017 bghe<!--Tested --> | |February 2017 bghe <!--Tested --> | ||
|- | |||
|BPSG low stress<!-- Recipe --> | |||
|302 nm/min<!-- Dep. rate [nm/min] --> | |||
|1.4598<!-- RI --> | |||
|± 1.7%<!-- Unif. [%] --> | |||
|Compressive: 1.4 MPa<!-- Stress [MPa] --> | |||
|Measured after anneal in Clad1000 <!-- Comments --> | |||
|17<!-- SiH4 [sccm] --> | |||
|1600<!-- N2O [sccm] --> | |||
|<!-- N2 [sccm] --> | |||
|240<!-- B2H6 --> | |||
|60<!-- PH3 --> | |||
|500 mTorr<!-- Pressure [mTorr] --> | |||
|800LF<!-- Power [W] --> | |||
|<!-- Load --> | |||
|<!-- Tune --> | |||
|10:00 <!-- Time [mm:ss] --> | |||
|February 2017 bghe <!--Tested --> | |||
|- | |||
|} | |||
*[[/conformity|SEM images of the conformity of the layer on a structured surface]] | |||
<br clear="all" /> | |||
=Recipes on PECVD3 for deposition of silicon oxides= | |||
{| border="1" cellspacing="2" cellpadding="2" colspan="3" | |||
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD3 - oxide''' | |||
|- | |||
| | |||
*[http://labmanager.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3 - requires login]<br> | |||
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3 - requires login] | |||
{| {{table}} | |||
| align="center" | | |||
{| border="1" cellspacing="1" cellpadding="2" align="center" style="width:200px" | |||
! QC Recipe: | |||
! QCOXYD2 | |||
|- | |||
| SiH<sub>4</sub> flow | |||
|12 sccm | |||
|- | |||
|N<sub>2</sub>O flow | |||
|1420 sccm | |||
|- | |||
|N<sub>2</sub> flow | |||
|392 sccm | |||
|- | |||
|Pressure | |||
|700 mTorr | |||
|- | |||
|RF-power | |||
|150 W | |||
|- | |||
|} | |||
| align="center" valign="top"| | |||
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px" | |||
!QC limits | |||
!PECVD3 - OXIDE | |||
|- | |||
|Deposition rate | |||
|97 - 112 nm/min | |||
|- | |||
|Non-uniformity | |||
|<2.0 | |||
|- | |||
|Refractive index | |||
|1.467 - 1.474 | |||
|- | |||
|} | |||
|- | |- | ||
|} | |||
|} | |} | ||
===Recipes=== | |||
{| border="1" cellspacing="0" cellpadding="7" | |||
|- | |||
|Recipe name | |||
|SiH4 flow [sccm] | |||
|N<sub>2</sub>O flow [sccm] | |||
|N2 flow [sccm] | |||
|B2H6 flow [sccm] | |||
|PH3 flow [sccm] | |||
|Pressure [mTorr] | |||
|Power [W] | |||
|Description | |||
|- | |||
|LFSiO2 | |||
|12 | |||
|1420 | |||
|392 | |||
|0 | |||
|0 | |||
|700 | |||
|150 | |||
|New QC implemented in April 2016 | |||
|- | |||
|LFSiO | |||
|12 | |||
|1420 | |||
|392 | |||
|0 | |||
|0 | |||
|550 | |||
|60 | |||
|Uniform silicon oxide | |||
|- | |||
|1PBSG | |||
|17 | |||
|1600 | |||
|0 | |||
|135 | |||
|40 | |||
|500 | |||
|800 LF | |||
|BPSG glass for waveguide cladding layer | |||
|} | |||
LF=Low Frequency | |||
===Expected results=== | |||
{| border="1" cellspacing="0" cellpadding="5" | |||
|- | |||
|Recipe name | |||
|Deposition rate [nm/min] | |||
|RI | |||
|Uniformity [%] | |||
|Stress | |||
|Comment | |||
|- | |||
|LFSiO2 | |||
|105nm/min | |||
|1.47 | |||
|~1.5% | |||
|'''400-402 MPa''' compressive stress '' by Anders Simonsen @nbi.ku.dk April 2016'' | |||
|We have seen that this recipe does not deposit the first minute | |||
|- | |||
|LFSiO | |||
|~75 | |||
|~1.48 | |||
|<1 | |||
|not measured | |||
|. | |||
|- | |||
|1PBSG | |||
|~228 nm/min | |||
|. | |||
|~17% | |||
|not measured | |||
|. | |||
|} | |||
<br clear="all" /> | <br clear="all" /> | ||
=Recipes on PECVD2 for deposition of silicon oxides= | =Recipes on PECVD3 for deposition of doped oxide= | ||
===Recipes=== | |||
{| border="1" cellspacing="0" cellpadding="7" | |||
|- | |||
|Recipe name | |||
|SiH<sub>4</sub> flow [sccm] | |||
|N<sub>2</sub>O flow [sccm] | |||
|N<sub>2</sub> flow [sccm] | |||
|GeH<sub>4</sub> flow [sccm] (scaled by 100) | |||
|B<sub>2</sub>H<sub>6</sub> flow [sccm] | |||
|PH<sub>3</sub> flow [sccm] | |||
|Pressure [mTorr] | |||
|Power [W] | |||
|Description | |||
|- | |||
|Core-Ge (not possible anymore as we have no Germanium) | |||
|17 | |||
|1600 | |||
|300 | |||
|300 | |||
|0 | |||
|0 | |||
|400 | |||
|600 LF | |||
|Process for germanium doped core layer developed by Haiyan Ou from DTU Photonics | |||
Annnealing: Anneal bond furnace, recipe "core1100" | |||
|- | |||
|Top-BPSG | |||
|17 | |||
|1600 | |||
|0 | |||
|0 | |||
|100 | |||
|40 | |||
|500 | |||
|800 LF | |||
|Process for PBSG top clading layer developed by Haiyan Ou from DTU Photonics | |||
Annnealing/oxidation: Anneal bond furnace, recipe "clad1000" | |||
|} | |||
===Expected results=== | |||
{| border="1" cellspacing="0" cellpadding="5" | |||
|- | |||
|Recipe name | |||
|Deposition rate [nm/min] | |||
|Refractive index | |||
|- | |||
|Core-Ge | |||
|~188 nm/min | |||
|~1.46969 | |||
|- | |||
|Top-BPSG | |||
|~248 nm/min | |||
|~1.458 | |||
|} | |||
=Recipes on PECVD2 for deposition of silicon oxides <span style="color:Red">EXPIRED!!!</span>= | |||
==Quality control recipe (recipe changed in June 2015)== | ==Quality control recipe (recipe changed in June 2015)== | ||
| Line 90: | Line 366: | ||
|- | |- | ||
| | | | ||
{| {{table}} | {| {{table}} | ||
| align="center" | | | align="center" | | ||
| Line 122: | Line 397: | ||
!PECVD2 | !PECVD2 | ||
|- | |- | ||
| | |Deposition rate of Silicon Oxide | ||
| | |58 nm/min - 78nm/min | ||
|- | |- | ||
|Non-uniformity of the deposition rate: ''(max-min)/2*AVG'' | |Non-uniformity of the deposition rate: ''(max-min)/2*AVG'' | ||
| Line 131: | Line 406: | ||
|1.45 - 1.48 | |1.45 - 1.48 | ||
|- | |- | ||
|Non-uniformity of the | |Non-uniformity of the refractive index: ''(max-min)/2*AVG'' | ||
|<0.2% | |<0.2% | ||
|- | |- | ||
| Line 139: | Line 414: | ||
|} | |} | ||
==SiO2, High Rate== | ==SiO2, High Rate <span style="color:Red">EXPIRED!!!</span>== | ||
| Line 165: | Line 440: | ||
|} | |} | ||
==SiO2 Low Rate== | ==SiO2 Low Rate <span style="color:Red">EXPIRED!!!</span>== | ||
| Line 257: | Line 532: | ||
<br clear="all" /> | <br clear="all" /> | ||
==BPSG: RI vs. B/P == | ==BPSG: RI vs. B/P <span style="color:Red">EXPIRED!!!</span> == | ||
B2H6 flow and PH3 flow was varied to map the RI of different B2H6/PH3 ratios. <br> | B2H6 flow and PH3 flow was varied to map the RI of different B2H6/PH3 ratios. <br> | ||
''Work done by BGHE@ | ''Work done by BGHE@dtu in fall 2013'' <br> | ||
{| border="1" cellspacing="0" cellpadding="7" | {| border="1" cellspacing="0" cellpadding="7" | ||
|- | |- | ||
| Line 333: | Line 608: | ||
<br clear="all" /> | <br clear="all" /> | ||
=Recipes on PECVD1 for deposition of silicon oxides <span style="color:Red">EXPIRED!!!</span>= | |||
=Recipes on PECVD1 for deposition of silicon oxides <span style="color:Red"> | |||
===Recipes=== | ===Recipes=== | ||
{| border="1" cellspacing="0" cellpadding="7" | {| border="1" cellspacing="0" cellpadding="7" | ||