LabAdviser/Technology Research/Fabrication of Hyperbolic Metamaterials using Atomic Layer Deposition/EMT Procces flow: Difference between revisions
Appearance
mNo edit summary |
|||
| (26 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/LabAdviser/Technology_Research/Fabrication_of_Hyperbolic_Metamaterials_using_Atomic_Layer_Deposition/EMT_Procces_flow click here]''' | |||
<i>This page is written by <b>Evgeniy Shkondin @DTU Nanolab</b> if nothing else is stated. <br> | |||
All images and photos on this page belongs to <b>DTU Nanolab</b> and <b>DTU Electro</b> (previous DTU Fotonik).<br></i> | |||
=Fabrication of Hyperbolic Metamaterials by ALD: Aluminum Oxide/Titanium Oxide Multilayers for EMT Application= | |||
The fabrication and characterization described below were conducted in <b>2013-2016 by Evgeniy Shkondin, DTU Nanolab</b>.<br> | |||
====Procces flow description==== | ====Procces flow description==== | ||
The substrates for the samples were fabricated by depositing 1 μm of Si<sub>3</sub>N<sub>4</sub> (the resonator layer) on 100 mm silicon < 100 > wafers using low-pressure chemical vapor deposition. The process was carried out at 780C with ammonia (NH<sub>3</sub>) and dichlorosilane (SiH<sub>2</sub>Cl<sub>2</sub>) as reactive gases. Thickness and refractive index of the deposited silicon nitride was measured and confirmed using spectroscopic ellipsometry. The deposited Si<sub>3</sub>N<sub>4</sub> film was carefully analyzed for existence of cracks, particles and other defects using dark field optical microscopy. The best-quality wafer with Si<sub>3</sub>N<sub>4</sub> was selected and cleaved in pieces, which were used as substrates for the deposition of Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers. Before inserting each substrate into the ALD reactor, it was placed on a Si carrier wafer. Therefore the Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers were grown not only on the Si<sub>3</sub>N<sub>4</sub> layer but also on the dummy carrier wafer. After the ALD process was completed, the dummy was cleaved and its cross-section was characterized using scanning electron microscopy (SEM). The SEM images reveal high-quality homogeneous, conformal coatings, as seen in the examples in Figs 1. Such a method of deposited multilayers characterization turned out to be more feasible than the direct SEM characterization of multilayers on Si<sub>3</sub>N<sub>4</sub>, since the latter suffers from issues related to charge accumulation on the silicon nitride. | The substrates for the samples were fabricated by depositing 1 μm of Si<sub>3</sub>N<sub>4</sub> (the resonator layer) on 100 mm silicon < 100 > wafers using low-pressure chemical vapor deposition. The process was carried out at 780C with ammonia (NH<sub>3</sub>) and dichlorosilane (SiH<sub>2</sub>Cl<sub>2</sub>) as reactive gases. Thickness and refractive index of the deposited silicon nitride was measured and confirmed using spectroscopic ellipsometry. The deposited Si<sub>3</sub>N<sub>4</sub> film was carefully analyzed for existence of cracks, particles and other defects using dark field optical microscopy. The best-quality wafer with Si<sub>3</sub>N<sub>4</sub> was selected and cleaved in pieces, which were used as substrates for the deposition of Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers. Before inserting each substrate into the ALD reactor, it was placed on a Si carrier wafer. Therefore the Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers were grown not only on the Si<sub>3</sub>N<sub>4</sub> layer but also on the dummy carrier wafer. After the ALD process was completed, the dummy was cleaved and its cross-section was characterized using scanning electron microscopy (SEM). The SEM images reveal high-quality homogeneous, conformal coatings, as seen in the examples in Figs 1. Such a method of deposited multilayers characterization turned out to be more feasible than the direct SEM characterization of multilayers on Si<sub>3</sub>N<sub>4</sub>, since the latter suffers from issues related to charge accumulation on the silicon nitride. | ||
<gallery caption="" widths="1000px" heights="700px" perrow="1"> | |||
image:multilayers222.jpg| Al<sub>2</sub>O<sub>3</sub>/TiO<sub>2</sub> multilayers. | |||
</gallery> | </gallery> | ||
== Process flow == | == Process flow == | ||
Description of process flow. | |||
{| border="1" cellspacing="1" cellpadding="3" style="text-align: left; width: 925px; height: 220px;" | {| border="1" cellspacing="1" cellpadding="3" style="text-align: left; width: 925px; height: 220px;" | ||
| Line 29: | Line 33: | ||
|- | |- | ||
! | !1.1 | ||
|Plasma surface treatment | |Plasma surface treatment | ||
|To ensure clean surface, the 100 mm Si wafer is treated by O<sub>2</sub>/N<sub>2</sub> plasma. | |To ensure clean surface, the 100 mm Si wafer is treated by O<sub>2</sub>/N<sub>2</sub> plasma. | ||
|[[Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_2| Plasma Asher 2]] | |[[Specific_Process_Knowledge/Lithography/Strip#Plasma_Asher_2| Plasma Asher 2]] | ||
| | |[[image:1_Si.JPG|250x350px|center|]] | ||
|- | |- | ||
|- | |- | ||
|- style="background:#BCD4E6; color:black" | |- style="background:#BCD4E6; color:black" | ||
! | !1.2 | ||
|Deposition of 1 µm Si<sub>3</sub>N<sub>4</sub> layer | |Deposition of 1 µm Si<sub>3</sub>N<sub>4</sub> layer | ||
|Deposition carries 7 times | |Deposition carries 7 times in order to get 1 µm thick film | ||
|[[Specific_Process_Knowledge/Thin_film_deposition/Furnace_LPCVD_Nitride/Deposition_of_stoichiometric_nitride_using_the_6"_LPCVD_nitride_furnace|6" LPCVD nitride furnace]]. | |[[Specific_Process_Knowledge/Thin_film_deposition/Furnace_LPCVD_Nitride/Deposition_of_stoichiometric_nitride_using_the_6"_LPCVD_nitride_furnace|6" LPCVD nitride furnace]]. | ||
|[[image: | |[[image:2_SiN_LPCVD.JPG|250x350px|center|]] | ||
|- | |- | ||
|- | |- | ||
! | !1.3 | ||
|Surface investigation using optical microscopy in dark field mode | |Surface investigation using optical microscopy in dark field mode | ||
|The best quility wafer selects and cleaves in four pieces. | |The best quility wafer selects and cleaves in four pieces. | ||
| [[Specific_Process_Knowledge/Characterization/Optical_microscope|Optical Microscopy]]. | | [[Specific_Process_Knowledge/Characterization/Optical_microscope|Optical Microscopy]]. | ||
|[[image: | |[[image:Captured_10x19_defects_in_SiN.jpg|250x350px|center|]] | ||
|- | |- | ||
|- | |- | ||
|- style="background:#BCD4E6; color:black" | |- style="background:#BCD4E6; color:black" | ||
! | !1.4 | ||
|TiO<sub>2</sub>/Al<sub>3</sub>O<sub>3</sub> multilayers deposition using Atomic Layer Deposition | |TiO<sub>2</sub>/Al<sub>3</sub>O<sub>3</sub> multilayers deposition using Atomic Layer Deposition | ||
|Deposition using recipies EMA01, EMA02, EMA03 and EMA04. | |Deposition using recipies <b>EMA01</b>, <b>EMA02</b>, <b>EMA03</b> and <b>EMA04</b>. | ||
|[[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200|ALD Picosun R200]], | |[[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200|ALD Picosun R200]], <b>EMA01-04</b> Recipes description and performance: [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/ALD_multilayers#Low_temperature_grown_multilayers_on_flat_surfaces|Multilayrs recipes and their performance]] . | ||
|[[image: | |[[image:3_ALD.JPG|250x350px|center]] | ||
|- | |- | ||
|- | |- | ||
! | !1.5 | ||
|Scanning Electron Microscopy inspection | |Scanning Electron Microscopy inspection | ||
|By cleaving the sample it is possible to inspect depositet ALD layers uniformity in cross-sectional mode | |By cleaving the sample it is possible to inspect depositet ALD layers uniformity in cross-sectional mode | ||
|[[ | | | ||
|[[image: | [[Specific_Process_Knowledge/Characterization/SEM_Supra_1|SEM Supra 1]] | ||
<br clear="all" /> | |||
[[Specific_Process_Knowledge/Characterization/SEM_Supra_2|SEM Supra 2]] | |||
<br clear="all" /> | |||
[[Specific_Process_Knowledge/Characterization/SEM_Supra_3|SEM Supra 3]] | |||
|[[image:multilayers222.jpg|250x350px|center]] | |||
|- | |- | ||
| Line 73: | Line 82: | ||
|- | |- | ||
|- style="background:#BCD4E6; color:black" | |- style="background:#BCD4E6; color:black" | ||
! | !1.6 | ||
| | |XPS inspection for elemental trace analysis | ||
| | |XPS can be used in depth profile mode. Ar<sup>+</sup> ions erodes the surface of multilayers, allowing the inspection of each layer. | ||
|| | ||Equipment used: [[Specific_Process_Knowledge/Characterization/XPS/K-Alpha|XPS K-Alpha]]. Results of depth profiling presented: [[Specific_Process_Knowledge/Thin_film_deposition/ALD_Picosun_R200/ALD_multilayers#Investigation_of_chemical_composition_in_multilayers_system| XPS results]] . | ||
|[[image: | |[[image:XPS_depth_Al_10_AL.jpg|250x350px|center]] | ||
|- | |- | ||