Al2O3 etching by sanvis@nanolab
Line 131: | Line 131: | ||
===Results=== | ===Results=== | ||
<gallery caption="Profile view" widths="400px" heights="325px" perrow="3"> | <gallery caption="Profile view, etch time 40 min, started with 380 nm zep resist" widths="400px" heights="325px" perrow="3"> | ||
Image:S038116_01.jpg | Image:S038116_01.jpg |
Revision as of 14:45, 22 November 2023
Feedback to this page: click here
Al2O3 etching with the ICP metal
Parameter | Recipe name: no name (testing recipe) |
---|---|
Coil Power [W] | 1200 |
Platen Power [W] | 200 |
Platen temperature [oC] | 0 |
BCl3 flow [sccm] | 60 |
Cl2 flow [sccm] | 30 |
Pressure [mTorr] | 4 |
Material to be etched | Etch rate using the above parameters |
---|---|
Al2O3 |
|
Al2O3 etching by sanvis@nanolab ![Section under construction.jpg](/images/thumb/9/9a/Section_under_construction.jpg/70px-Section_under_construction.jpg)
Presentation made by Sanvis @DTU Nanolab
Parameter | Nanoscale Al2O3 etch | Microscale Al2O3 etch |
---|---|---|
Coil Power [W] | 300 | 500 |
Platen Power [W] | 15 | 70 |
Platen temperature [oC] | 0 | 0 |
BCl3 flow [sccm] | 20 | 40 |
Cl2 flow [sccm] | 7 | 15 |
Pressure [mTorr] | 1.2 | 3.0 |
Material to be etched | Nanoscale Al2O3 etch | Microscale Al2O3 etch |
---|---|---|
Etch rate | 6.25 nm/min on 6" wafer, Summer sanvis@nanolab | 25 nm/min on small samples on Si carrier, Summer 2022 sanvis@nanolab |
Al2O3 etching by bghe@nanolab
Recipes
Parameter | Recipe 1:Al2O3 etch platen only |
---|---|
BCl3 (sccm) | 15 |
Ar (sccm) | 15 |
Pressure (mTorr) | 5 |
Coil power (W) | 0 |
Platen power (W) | 30 |
Temperature (oC) | 20 |
Spacers (mm) | 100 mm |
Results
- Profile view, etch time 40 min, started with 380 nm zep resist
- Top view after resist strip