SEM images showed about 1.55µm – so it seems like ScanAsyst is pressing a little down in the resist compared with the SiO2 giving a too small height difference. | SEM images showed about 1.55µm – so it seems like ScanAsyst is pressing a little down in the resist compared with the SiO2 giving a too small height difference. | ||
Therefor When scanning steps with difference materials, when one of the materials is soft and you need to know the height difference, then it seems to be best to use tapping mode. | Therefor When scanning steps with difference materials, when one of the materials is soft and you need to know the height difference, then it seems to be best to use tapping mode. | ||
We did not save the images. Therefor I remeasured a few days later: | |||
====Tapping mode with TAP150A==== | |||
*CL on | |||
*256*32 | |||
*0dg | |||
*Step height: 1545/1532 nm | |||
====ScanAsyst with TAP150A==== | |||
*CL on | |||
*256x32 | |||
*0dg | |||
*ScanAsyst noise threshold: 1 | |||
*PeakForce amplitide 75 nm (was set as standard from the probe settings) | |||
*Peak force frequency: 2 Hz | |||
*Step height: 1537 nm | |||
====ScanAsyst with ScanAsyst-air==== | |||
*CL on | |||
*256x32 | |||
*0dg | |||
*ScanAsyst noise threshold: 1 | |||
*PeakForce amplitide 150 nm (I had to increase it from the 75 nm) | |||
*Peak force frequency: 2 Hz | |||
*Step height: 1545 nm | |||
====Tapping mode with RFESP-75==== | |||
*CL on | |||
*256*32 | |||
*0dg | |||
*Step height: 1525 nm | |||