Phosphorous doped poly silicon by using B4 4" LPCVD polysilicon furnace
Result from Niccolò Bottauscio, DTU Nanolab, November 2025
In order to check the deposition rate, uniformity and sheet resistance for phosphorous doped polySi, a deposition has been done using the standard recipe "POLYPH3" with the standard temperature, pressure and gas flow settings and with three oxidized 4" Si test wafers distributed over the quartz boat in the furnace.
The thickness of the deposited polySi layer has been measured, and the deposition rate has been calculated. The sheet resistance has also been measured.
Afterwards, the wafers have been annealed in the C4 Al-Anneal furnace.
Process
PolySi deposition parameters:
- Recipe: "POLYPH3"
- Deposition time: 2 hours
- Temperature: 525 °C (zone 1), 518 °C (zone 2), 525 °C (zone 3)
- Pressure: 200 mtorr
- Silane (SiH4) flow: 80 sccm
- Phosphine (PH3)/N2 flow: 7 sccm
Wafers
- Test wafers:
- w6 (towards furnace), w15 (center), w24 (towards door)
- Oxide thickness: 472 nm
- The wafer flat was pointing upwards in the furnace boat
- Dummy wafers: w1 - w5, w7 - w14, w16 - w23, w25 - w26
Annealing parameters
- Recipe: "Ann1000"
- Annealing time: 1 hour
- Temperature 1000 °C
Results - Before annealing
An image of one of the test wafers after the deposition can be seen here:
From the image it can be seen that the color and thus the phosphorous doping is not very uniform over the entire wafer surface. However, if the edge of the wafer is excluded, a good uniformity is actually obtained.
The thickness of the deposited phosphorous doped polySi layer has been measured in five points over each of the three test wafers using the Ellipsometer VASE.
| Ellipsometer measurements of the phosphorous doped polySi thickness [nm] | ||||
|---|---|---|---|---|
| Test wafer number | w6 | w15 | w24 | |
| Ellipsometer measurement
points (x [cm], y [cm]) and thickness [nm] | ||||
| (0,0)
Wafer center |
102.5 | 98.6 | 96.2 | |
| (-4,0) | 111.6 | 105.0 | 104.0 | |
| (0,4)
Wafer top/flat |
115.9 | 106.7 | 103.1 | |
| (-4,0) | 110.9 | 105.2 | 105.6 | |
| (-4,0)
Wafer bottom |
102.5 | 100.5 | 101.3 | |
| Average thickness [nm] | 108.7 | 103.2 | 102.0 | |
From the average thickness, the average deposition rate for each of the three test wafers has been calculated.
| Deposition rate for the phosphorous doped polySi | |||
|---|---|---|---|
| Test wafer number | w6 | w15 | w24 |
| Deposition rate | 0.91 nm/min | 0.86 nm/min | 0.85 nm/min |
The deposition rate is much slower than the deposition rate for undoped polySi. The reason for this is that the phosphorous passivates the wafer surface and thus slows down the deposition. This also explains the non-uniformity of the deposited layer. Furthermore, phosphorous doped polySi becomes poly-crystalline at lower temperatures than undoped polySi.
The sheet resistance has also been measured on the three test wafers. The measurements have been done in three points on each wafer using the 4-point probe Jandel.
| 4-point probe measurements of the the sheet resistance [kOhm/sq] | ||||
|---|---|---|---|---|
| Test wafer number | w6 | w15 | w24 | |
| 4-point probe
measurement points and sheet resistance [kOhm/sq] | ||||
| Wafer top/flat | 1.38 | 1.45 | 1.48 | |
| Wafer center | 1.48 | 1.51 | 1.51 | |
| Wafer bottom | 1.51 | 1.54 | 1.52 | |
| Average sheet resistance [kOhm/sq] | 1.44 | 1.50 | 1.52 | |
Results - After annealing
After the deposition, the three test wafers have been annealed in the C4 Al-Anneal furnace. The annealing parameters can be seen above.
After the annealing, the sheet resistance has again been measured in three points on each test wafer using the 4-point probe Jandel.
From the measurement results it can be seen that the annealing decreases the sheet resistance by around one order of magnitude.
| 4-point probe measurements of the the sheet resistance [Ohm/sq] | ||||
|---|---|---|---|---|
| Test wafer number | w6 | w15 | w24 | |
| 4-point probe
measurement points and sheet resistance [Ohm/sq] | ||||
| Wafer top/flat | 172 | 193 | 200 | |
| Wafer center | 187 | 199 | 206 | |
| Wafer bottom | 190 | 199 | 201 | |
| Average sheet resistance [Ohm/sq] | 183.0 | 197.0 | 202.3 | |