Specific Process Knowledge/Etch/ICP Metal Etcher/silicon oxide/By BGHE

From LabAdviser
Jump to navigation Jump to search

This page is written by Berit Herstrøm @ DTU Nanolab (BGHE) if nothing else is stated
I (bghe@nanolab 2016) tried with two different gas regimes: CF4 and C4F8. I only made a few tests with CF4 since I got a very bad selectivity to the resist mask and I dicided to go for the C4F8 instead.
Zhibo Li @ Danchip has also tried (December 2016) with similar setting, see his results in this file: File:Zhibo Li SiO2 ICP etch (dose205).docx

C4F8

Unless otherwise stated, all content in this section was done by Berit Herstrøm, DTU Nanolab
I started out with a recipe developed by Peixiong called pxSiO2try9, look at his results here

Parameter Mask material Barc etch Coil power Platen power Pressure Flow rate C4F8 Flow rate H2 Flow rate Ar T Process time Comment Results CD change (mask 55% trench) after s007467 is it <50% after barc etch

trench opening as a fraction of pitch

Profile angles Etch depth in SiO2 Etch rate Etch depth in resist Selectivity (resist:SiO2) Etch rate in Si
s008684 880nm KRF barc etch CF 50s 1000W 200W 2.5mTorr 13sccm 30sccm 0 0 1:30min The layer in this case is 300nm Si3N4

S008684 Si3N4 19.jpg S008684 Si3N4 20.jpg

35% (1µm pitch)
47% (6µm pitch)

83-88

>300nm/min (Si3N4)

240nm

~1:2 (Si3N4)

?

s007785 880nm KRF pxbarcO2 25s 800W 200W 2.5mTorr 13sccm 26sccm 0 0 7 min One of the good ones. the mask is well preserved

S007785 05.jpg S007785 08.jpg

37% (1µm pitch)
48% (4µm pitch)

83-86

>1000 nm

>143nm/mi

250nm

>1:4

?

s007679 880nm KRF barc etch CF 40s 800W 200W 2.5mTorr 13sccm 26sccm 0 0 8 min One of the good ones. the mask is well preserved, CF barc etch

ICP metal s007679 01.jpg ICP metal s007679 04.jpg

42% (1µm pitch)
48% (4µm pitch)

83-89

>1074 nm

>134nm/min

310nm

>1:3.5

?

s007592 880nm KRF barc etch CF 40s 1000W 200W 2.5mTorr 10sccm 28sccm 0 0 5 min One of the good ones. the mask is well preserved, CF barc etch

ICP metal s007592 21.jpg ICP metal s007592 24.jpg

41% (1µm pitch)
47% (4µm pitch)

86-87

727 nm (1µm)
864 nm (4µm)

145 nm/min (1µm pitch)
172 nm/min (4µm pitch

170nm

1:4.3 (1µm P)
1:5.1 [4µm P)

?

s007593 880nm KRF barc etch CF 40s 800W 100W 2.5mTorr 10sccm 28sccm 0 0 8 min One of the good ones. the mask is well preserved, CF barc etch. The small pitch line are etched much slower that the higher pitch lines

ICP metal s007593 25.jpg ICP metal s007593 28.jpg

32% (1µm pitch)
45% (4µm pitch)

85-86

501 nm (1µm)
881 nm (4µm)

63 nm/min (1µm pitch)
110 nm/min (4µm pitch

100nm

1:5.0 (1µm P)
1:8.8 [4µm P)

?

s007467 (as 18) 750nm KRF none 1000W 150W 2.5mTorr 8sccm 30sccm 0 0 10min

ICP metal s007467 07.jpg ICP metal s007467 09.jpg

? (2µm pitch)
52% (average) (3µm pitch)
51% (average) (6µm pitch)

77 (6µm p)

1015 nm (2µm pitch)
1032 nm (3µm pitch)
1060 nm (6µm pitch)

101.5 nm/min (2µm pitch)
103.2 nm/min (3µm pitch)
106.0 nm/min (6µm pitch)

210nm

1:4.8 (2µm pitch)
1:4.9 (3µm pitch)
1:5.0 (6µm pitch)

s007418 750nm KRF none 1000W 150W 2.5mTorr 8sccm 30sccm 0 0 5min

ICP metal s007418 09.jpg ICP metal s007418 12.jpg

46.5% (2µm pitch)
49.0% (4µm pitch)

87-88 (large structures)

400 nm (6µm pitch)

80 nm/min (6µm pitch)

200nm/76nm?

1:2 (6µm pitch)
1:5?


s007565 (as 16) 880nm KRF barc etch CF 40s 800W 100W 2.5mTorr 13sccm 26sccm 0 0 8min repeated s007416 and s007468 with a barc etch step. This improved the uniformity of the etch performance over different linewidth and improved the selectivity to the mask and the profile angle. After this I continued with barc etch. Nice

ICP metal s007565 02.jpg ICP metal s007565 06.jpg

44.5% (2µm pitch)
46.8% (3µm pitch)
47.8% (4µm pitch)

87-88

779 nm (2µm pitch)
862 nm (3µm pitch)
854 nm (4µm pitch)

97.4 nm/min (2µm pitch)
107.8 nm/min (3µm pitch)
106.8 nm/min (4µm pitch)

130nm

1:6.0 (2µm pitch)
1:6.6 (3µm pitch)
1:6.6 (4µm pitch)

s007468 (as 16) 750nm KRF none 800W 100W 2.5mTorr 13sccm 26sccm 0 0 10min Repeated s007416 with double time.

ICP metal s007468 12.jpg ICP metal s007468 15.jpg

17.3% (1µm pitch)
33.5% (2µm pitch)
38.3% (3µm pitch)
41.4% (4µm pitch)

76-78

850 nm (1µm pitch)
1034 nm (2µm pitch)
1048 nm (3µm pitch)
1055 nm (4µm pitch)

85 nm/min (1µm pitch)
103.4 nm/min (2µm pitch)
104.8 nm/min (3µm pitch)
105.5 nm/min (4µm pitch)

300nm

1:2.8 (1µm pitch)
1:3.4 (2µm pitch)
1:3.5 (3µm pitch)
1:3.5 (4µm pitch)

s007416 750nm KRF none 800W 100W 2.5mTorr 13sccm 26sccm 0 0 5min From S007411 the platen power was decreased to avoid trenching. The etch rate went down and some variation in profile angle is seen from small opening to large opening. Started plasma on the 4th try

ICP metal s007416 05.jpg ICP metal s007416 06.jpg

38.6% (2µm pitch)
45.4% (5µm pitch)

77 (small structures) 90 (large structures)

346 nm (1.5µm pitch)
454 nm (5µm pitch)

69 nm/min (1.5µm pitch)
91 nm/min (5µm pitch)

50nm

1:7 (1.5µm pitch)
1:9 (5µm pitch)


s007411 750nm KRF none 800W 150W 2.5mTorr 13sccm 26sccm 0 0 5min From s007409 the Gas flow ratio between C4F8 and H2 has been changed to more C4F8 and less H2. This increased the etch rate (more fluorine). Trenching is seen and tappered sidewall is seen indicating a more physical etch.

ICP metal s007411 01.jpg ICP metal s007411 02.jpg

47.0% (1µm pitch)
44.6% (2µm pitch)

83

708 nm

142 nm/min

294 nm

1:2.4

s007419 750nm KRF none 800W 200W 2.5mTorr 8sccm 30sccm 0 0 5min Increased the platen power. The selectivity and profile looks good but the resist profile has been rounded more on the edge and this will effect the profile for a deeper etch.

ICP metal s007419 17.jpg ICP metal s007419 21.jpg

46.6% (1µm pitch)
47.8% (2µm pitch)
48.4% (4µm pitch)

86-90

270nm (1µm pitch)
400nm (2.5µm pitch)

54 nm/min (1µm pitch)
80 nm/min (2.5µm pitch)

100nm

1:4 (2.5µm pitch)

s007410 750nm KRF none 800W 75W 2.5mTorr 8sccm 30sccm 0 0 7min Reduced the platen power.Effect: ARDE - less CD increase but more possitive tappered profile.

ICP metal s007410 05.jpg ICP metal s007410 09.jpg

42.3% (2µm pitch)
47.0% (average) (3µm pitch)

80-82

0 nm (1µm pitch)
270 nm (3µm pitch)

0 nm/min (1µm pitch)
39nm/min (?µm pitch)

100nm

1:0 (1µm pitch)
1:2.7 (2µm pitch)

s006656 750nm KRF none 1000W 150W 2.5mTorr 15sccm 0sccm 30sccm 0 10min Tried with C4F8/Ar instead of C4F8/H2 => much lower etch rate and bad selectivity to the resist.

ICP metal s006656 no1.jpg ICP metal s006656 no2.jpg

358 nm

35.8 nm/min (2µm pitch)

526nm

1:0:68

s007409 750nm KRF none 800W 150W 2.5mTorr 8sccm 30sccm 0 0 5min Repeated Pexiongs recipe without barc etch and only 5 min's runs. It probably takes about 1 min to get through the barc. If you count that in then the etch rate and relectivity to resist is almost the same as for the first run. Effect: CD increase

ICP metal s007409 06.jpg ICP metal s007409 07.jpg

47.4% (1µm pitch)
47.5% (2µm pitch)
50.0% (3µm pitch)

86-89

280 nm (1µm pitch)
370 nm (2µm pitch)

56 nm/min (1µm pitch)
74 nm/min (2µm pitch)

160nm

1:1.8 (1µm pitch)
1:2.3 (2µm pitch)

s006106 750nm KRF Barc etch O2 75s 800W 150W 2.5mTorr 8sccm 30sccm 0 0 10min From Peixiong

S0061066 n02.jpg S006106 n04.jpg

60%

79

1053 nm (center)
1043 nm (edge)

105 nm/min

280nm

1:3:75 (2µm pitch)

CF4

I stopped trying with CF4 because I got bad selectivty to the resist and decided to focus on the recipe with C4F8 instead.

Parameter/Wafer ID s006687 s006701 s007258 s007350 s007352
Mask material 750nm KRF 750nm KRF 750nm KRF 750 nm KRF 750nm KRF
Barc etch none none none none none
Coil power 800W 800W 800w 800w 800w
Platen power 100W 100W 100w 60W 30w
Pressure 4mTorr 4mTorr 4mTorr 4mTorr 4mTorr
Flow rate CF4 20sccm 25sccm 30sccm 30sccm 30sccm
Flow rate H2 20sccm 15sccm 10sccm 10sccm 10sccm
T 0 0 0 0 0
Process time 10min 10min 2min30 2min30 3min30
Comment Little resist left, Trenching A little trenching very little trenching in large lines - anti trenching in small lines
Results
profile near edge
Profile near middel
tilted
profile
s007350 2µm pitch
s007350 2µm pitch
s007350 1µm pitch
s007352 1µm pitch
s007352 2µm pitch
Etch depth in SiO2 374nm 505nm 578nm 336nm 235nm
Etch rate 37.4nm/min 50.5nm/min 231nm/min 134.4nm/min 88nm/min
Etch depth in resist 345nm 633nm 700nm 405nm 308nm
Selectivity (resist:SiO2) 1:1.1 1:0.80 1:0.83 1:0.83 1:0.76