Nano scale etching of silicon nitride with SF6 plasma

Based on silicon etch recipe made by Henri Jansen.

silicon nitride etch
Parameter Silicon nitride etch, platen only
SF6 (sccm) 5
Pressure (APC %) 100
Platen power (W) 20
Temperature (oC) 20

The recipe was tested by Marcus Hufe, July 2024

A full 100 mm wafer was etched on top of a 150 mm silicon wafer. The etch depth was measured by AFM to check for etch depth etch depth uniformity over the wafer:

  • Center: 25 nm, delta 1½ nm (+/-)
  • North: 25 nm d 1 nm
  • South: 24 nm d 1 nm
  • East: 24.5 d 1 nm
  • West: 24 d 1 nm