Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)/Remove resist in the AOE
Appearance
- Feedback to this page: click here
Remove AZ resist in the AOE using the recipe Descum
| Parameter | Descum |
|---|---|
| Coil Power [W] | 2000 |
| Platen Power [W] | 30 |
| Platen temperature [oC] | 0 |
| O flow [sccm] | 99 |
| Pressure [mTorr] | 10.0 (strike pressure 20.0 mTorr) |
| Typical results | tested by bge@danchip |
|---|---|
| AZ resist etch rate | ~41 nm/s |
BARC etching
I have tried once etching BARC with recipe m_res_ny:
| Parameter | Resist mask |
|---|---|
| Coil Power [W] | 1300 |
| Platen Power [W] | 200 |
| Platen temperature [oC] | 0 |
| He flow [sccm] | 174 |
| CF flow [sccm] | 5 |
| H flow [sccm] | 4 |
| Pressure [mTorr] | 4 |
| Etch rate in BARC [nm/sec] | 2 |