Nominal trench line width ' ' 30 60 90 120 150 Average Std. dev.
Etch rate nm/min 59 67 67 67 68 66 4
Sidewall angle degs 84 86 84 86 86 85 1
CD loss nm/edge -16 -31 -29 -36 -33 -29 8
CD loss foot nm/edge -16 -23 -14 -18 -12 -17 4
Bowing 7 23 15 10 9 13 7