Trial runs on HTF stepper wafers 22/6-2012

Process conditions
Substrate information Wafer S002872
Substrate description 200 nm wide trenches with 400 nm pitch in Barc+stepper resist on quarter 6" wafer CB on oxide carrier
Date 22/6-2012
Tool Pegasus
Process Recipe nb-1.0
Tool conditioning TDESC clean (?) then 30 second barc etch step before etch
Process duration 3:45 minutes
Purpose test
Characterisation SEM Zeiss


Improved matching 11/9-2012

Process conditions
Substrate information Wafer S003051
Substrate description 200 nm wide trenches with 400 nm pitch in Barc+stepper resist on quarter 6" wafer CB on oxide carrier
Date 11/9-2012
Tool Pegasus
Process Recipe nb-1.0
Tool conditioning TDESC clean (?) then 30 second barc etch step before etch
Process duration 8:00 minutes or 60 cycles
Purpose Improved matching
Characterisation SEM Zeiss


Test run on AZ resist to see if it behaves well, 21/9-2012

Process conditions
Substrate information Wafer C01290.03
Mask 2.2 µm AZ resist
Date 21/9-2012
Tool Pegasus
Process Run ID C12090.03
Tool conditioning 5 minute TDESC clean
Mask description Travka50 mask
Purpose See how the nb-1.0 behaves on AZ resist
Characterisation SEM Leo