Process parameters for the acceptance test
| Parameter | Ti etch acceptance |
|---|---|
| Neutalizer current [mA] | 450 |
| RF Power [W] | 800 |
| Beam current [mA] | 400 |
| Beam voltage [V] | 500 |
| Beam accelerator voltage | 500 |
| Ar flow to neutralizer [sccm] | 5.0 |
| Ar flow to beam [sccm] | 10.0 |
| Rotation speed [rpm] | 20 |
| Stage angle [degrees] | 5 |