Specific Process Knowledge/Characterization/Profiler/Optical Profiler (Sensofar) acceptance test
Appearance
Results from the Optical Profiler (Sensofar) acceptance test
The acceptance test was performed in January 2012 by STInstruments and Sensofar together with Pernille V. Larsen @ Danchip and Berit G. Herstrøm @ Danchip.
This Table shows the accpetance criteria
| ' | Title | Sample description / measurement | Acceptance criteria |
| 1 | Patterned flat sample of silicon | Sample material: Patterned silicon substrate. | Depth 100±2 µm |
| Trench depth with aspect ratio 1:10 on a 10 µm wide trench | |||
| 2 | Patterned flat sample of silicon. | Sample material: Patterned silicon substrate. | Depth 91±2 µm |
| Trench depth with aspect ratio 1:11 on a 8 µm wide trench | |||
| 3 | Patterned flat sample of silicon | Sample material: Patterned silicon substrate | Depth 85±2 µm |
| Trench depth with aspect ratio 1:13 on a 6.4 µm wide trench | |||
| 4 | Patterned flat sample of glass | 3D profile of pattern etched down in a quartz sample. | Depth within ±1% from a standard profiler measurement and repeatability (3 successive measurements) within 0.1% |
| Pattern size 20 µm x 20 µm, depth 500 nm | |||
| 5 | Flat sample of silicon with thick patterned oxide | Step height of patterned thick (10 µm) oxide on top of a silicon wafer. | Step height must be within ±3% of a SEM profile measurement. |
| 7 µm deep pattern, trench width 6 µm | |||
| 6 | Flat sample of silicon with thick layer of patterned polymer | Sample material: SU8 on silicon. | Height 69±2 µm |
| Pillar heights of 69 µm with 25 µm between pillar edges | |||
| 7 | Free standing structure | Measure bow due to stress of a membrane. | Membrane bow repeatability of 5 successive measurement within 2% |
| Membrane material: Si(2 µm)/SiO2(~1 µm)/Au(50 nm). | |||
| Membrane size: honey comb structure approximately 150 µm in diameter. | |||
| Bow < 500 nm | |||
| 8 | Stitching of large area | Stitching 4 mm x 4 mm on same sample as in 7. The area consists of many closed packed honey comb formed membranes. | Membrane bow must the same as on 7 within 2% |
| 9 | Narrow trenches and holes | Sample material: Patterned silicon substrate. | Depth 20±2 µm |
| 2.5 µm wide trench in silicon with a depth of 20 µm | |||
| 10 | Film thickness measurement of transparent thin film | Transparent thin film thickness of 28 nm SiO2 on Si | SiO2 thickness 28±1 nm |
| 11 | Measurements of multiple stacks | 120 nm nitride on 110 nm oxide on a silicon substrate | Within ±2% on each layer from an ellipsometer measurement. |
| 12 | Film thickness measurements of transparent films on small structure | Sample material: Si with 1.5 µm patterned AZ-resist | Within ±1% from a standard profiler measurement. |
| Measure thickness of AZ-resist on pillars of 50 µm in diameter | |||
| 13 | Roughness repeatability | Sample material: Si wafer with poly-silicon layer. | Repeatability within 0.2% |
| 3 successive measurements of the roughness |
Results
Results of acceptance test no. 1
Sample material: Patterned silicon substrate Measurement: Trench depth with aspect ratio 1:10 on a 10 µm wide trench Acceptance criteria:Depth 100±2 µm
It was done in two ways:
- With confocal objective EPI 100x-N: See the results here
- With Interferometric objective 50X DI: See the results here
Setting for methode no. 1: confocal
Recipe: Trench
- Operation mode: trench
- + Raw smoothing confocal
- + fine shift
- Objective: EPI 100X-N
- Z scan
- Dual - bottom up
- top: 8µm
- Gap: 91µm
- Bottom: 8µm
- Speed factor: 1x
- + Linear stage
- Dual - bottom up
- Threshold: 0.0%
- Light source
- Levels: 2
- 900 -> 60
- Gain: default
- Levels: 2
Setting for methode no. 2: interferometric
We do not have a recipe for that but we used:
- Objective: Interferometric 50x DI
- Z scan: VSI
- Light souce: increased gain and contrast
Results of acceptance test no. 4
Sample material: Patterned fused silica. Measurement: Depth of pattern Acceptance criteria:Depth within ±1% from a standard profiler measurement and repeatability (3 successive measurements) within 0.1%
Standard profiler measurement: