Jump to content

Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300/Etch slow

From LabAdviser

Etch slow

This process development is going on to find an etch recipe that is so gentle that the resist masking material can be removed with acetone + ultrasound within hopefully 10min. This is important when a metal is to be etched as this cannot withstand plasma ashing (to remove reist mask) after the etch.

Parameter Si etch test1 Si etch test2
Neutalizer current [mA] 450 250
RF Power [W] 1200 1000
Beam current [mA] 400 200
Beam voltage [V] 400 200
Beam accelerator voltage 400 200
Ar flow to neutralizer [sccm] 6.0 6.0
Ar flow to beam [sccm] 6.0 6.0
Rotation speed [rpm] 20 20
Stage angle [degrees] 10 10
Platen temp. [dg. Celcius] 15 15
He cooling pressure [mTorr] 37.5 37.5
Results vvv
Etch time [min] 40 40
Etch rate in Si [nm/min] 19.7 3.58
Total time in Acetone + ultrasound [min] 17 10
Was the resist completely removed after acetone + ultrasound? no yes