Acceptance test for TiO2 deposition:

. Acceptance Criteria

Acceptance Results recipe 1

Acceptance Results recipe 2
Substrate information
  • 50 mm SSP Si wafer
  • 525 µm thick
  • Supplied by Danchip
  • 100 mm SSP Si wafer
  • 525+-25 µm thick
  • 100 mm SSP Si wafer
  • 525+-25 µm thick
Material to be deposited
  • TiO2

The purpose of the TiO2 is to be part of a mirror: <br\> 5 quarterwavelength pairs of <br\> SiO2 <br\> TiO2 <br\> Extra quarterwavelength layer of <br\> TiO2 <br\> 5 quarterwavelength pairs of <br\> SiO2 <br\> TiO2 <br\> Design wavelength (for refractive indices and layer thicknesses):1300nm <br\> The acceptance criteria is set up for the single SiO2 and TiO2 layers. <br\> Five runs in a row for each material.

  • TiO2
  • TiO2
Deposition thickness
  • 147nm
  • ~184 nm
  • 121 nm
Deposition rate
  • 2.8 nm/min
  • 3.54nm/min +- 0.03nm/min

One stdev - wafer to wafer

  • 3.03nm/min

Only done once

Thickness uniformity
  • <+-1%
  • <+-1.00%
  • <+-0.90%
Reproducibility
  • <+-1.5%
  • +-0.9% on 5 wafers in a row
  • not tested
Stress
  • <500MPa
  • ~300MPa
  • Not measured expect ~300MPa


Recipe 1 Recipe 2
Platen angle 50 degrees 30 degrees
Platen rotation speed 20rpm 20rpm
Ar(N) flow 4 sccm 4 sccm
Ar(dep. source) flow 9 sccm 9 sccm
O2(dep. source) flow 2 sccm 2 sccm
O2(etch source) flow 8 sccm 8 sccm
I(N) 459mA 450mA
Power 875W 875W
I(B) 390mA 390mA
V(B) 1300V 1300V
Vacc(B) 400V 400V



Other results

Roughness of the surface

Measured with the Optical profiler - PSI mode (on one sample from the acceptace test): Sa= ~1nm