Nanoetch in quartz 65mmx65mmx6.25mm substrates

by bge@danchip

Some priliminary results

The tests were done on 2" quartz wafers with a thickness of 1mm. These were placed on a 65mmx65mmx6,25mm quartz plate with a 2" groove. This 65mmx65mmx6,25mm plate was placed on a 4" Si wafer with a 65mmx65mm groove. the masking material was Cr sputter deposited in Wordentec and and patterned with ZEP520A resist by e-beam and ICP metal Cr etch.

Recipe used STS65x65:

Parameter Crom mask
Coil Power [W] 1200
Platen Power [W] 500
Platen temperature [oC] 50
CF4 flow [sccm] 43
C4F8 flow [sccm] 20
O2 flow [sccm] 10
Pressure [mTorr] 8


Parameter Results
Etch rate ~300nm/min
Etch profile 86-87 degrees
ARDE There does not seem to be a significant aspect ratio dependency in the etch rate up to aspect ratio 1:2 ~ 1:3
Mask selectivity 20nm Cr is enough to etch 200nm in the quartz
Images .


I am currently working on getting the right images in: 6. Jan 2012 /BGE

 
Process date: August 2011
Recipe: STS65x65@50degrees
Process time: 40sec.
Mask: Cr ~20nm thick
Design line width: 50nm Design periode: 150nm
 
Process date: August 2011
Recipe: STS65x65@50degrees
Process time: 40sec.
Mask: Cr ~20nm thick
Design line width: 75nm Design periode: 225nm
 
Process date: August 2011
Recipe: STS65x65@50degrees
Process time: 40sec.
Mask: Cr ~20nm thick
Design line width: 100nm Design periode: 300nm
 
Process date: August 2011
Recipe: STS65x65@50degrees
Process time: 40sec.
Mask: Cr ~20nm thick
Design line width: 200nm Design periode: 600nm
 
Process date: August 2011
Recipe: STS65x65@50degrees
Process time: 40sec.
Mask: Cr ~20nm thick
Design line width: 300nm Design periode: 900nm