Jump to content

Specific Process Knowledge/Thin film deposition/ALD2 (PEALD)/TiN deposition using ALD2

From LabAdviser
Revision as of 18:03, 5 October 2026 by Eves (talk | contribs) (→TiN thermal Nanolab Standard)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)

Feedback to this page: click here

This page is written by DTU Nanolab internal

This page is written by Evgeniy Shkondin @DTU Nanolab if nothing else is stated.
All images and photos on this page belongs to DTU Nanolab.
The fabrication and characterization described below were conducted in 2017 - 2021 by Evgeniy Shkondin, DTU Nanolab.

The initial results tested in 2017 can be found here.


Deposition of TiN is a standard, well-explored ALD process. In any book where ALD is explained or scientific reviews on a subject, the TiN process is mentioned as a standard example of nitride deposition with the corresponding reaction mechanism. In any facility with an ALD tool, you will also find a TiN process, since the film is popular in many applications because of its ease of deposition, excellent uniformity, strict thickness control, and reliability. At DTU Nanolab, you can use ALD-2 for the deposition of TiN with thermal or plasma methods.

TiN ALD deposition using TiCl4 and NH3

Thermal TiN can be deposited in the range between 450 °C to 500 °C.

TiN recipes

TiN thermal Nanolab Standard

Maximum deposition thickness: 100 nm

Temperature: 450 °C - 500 °C

TiCl4* NH3
Nitrogen flow 80 sccm 100 sccm
Pulse time 0.1 s 4.0 s
Purge time 5.0 s 8.0 s

This is a standard recipe of thermal TiN. It is suitable for coating the flat samples and structures with an aspect ratio of around up to 1:20.

Deposition characteristics

The deposition rate for TiN depends on the temperature, see the ALD-window graph below. The uniformity, thickness, refractive index has been obtained using Ellipsometer VASE.

Deposition rate

Uniformity

Sample Minimum thickness (nm) Maximum thickness (nm) Average thickness (nm) Standard deviation Uniformity (%)
500°C / 1300 cycles 29.21 39.20 32.51 2.49 15.37
500°C / 2300 cycles 56.75 76.39 62.64 5.18 15.67
500°C / 3300 cycles 82.99 107.45 92.25 6.88 13.26
500°C / 4300 cycles 107.56 141.44 118.86 8.92 14.25
500°C / 5300 cycles 133.53 180.00 148.38 12.96 15.66
500°C / 6300 cycles 169.57 250.00 210.46 31.01 19.11


Sheet resistance

Annealing

SEM

Cross-section of flat samples

Flat samples

HARS

Roughness

Optical functions

500 °C

450 °C

Transmission function

X-ray photoelectron spectroscopy

Effect of temperature

Stoichiometry results for TiN deposited with TiCl4 and NH3 thermal process.
Temperature °C 500 450 400 400 (LET*) 350
Ti (At. %) 45.30 44.63 44.37 44.46 44.40
N (At. %) 38.99 38.62 36.18 37.53 34.35
O (At. %) 15.71 15.27 15.97 15.27 16.76
Cl (At. %) 0 1.47 3.48 2.74 4.49

*LET - Longer exposure time of NH3 (5s)



Effect of annealing

Surface

Depth