Jump to content

Specific Process Knowledge/Lithography/Strip/plasmaAsher04

From LabAdviser
Revision as of 08:55, 25 June 2026 by Jehem (talk | contribs) (→Process development sections)
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)

Plasma Asher 4

 
Plasma asher 4 in cleanroom E-5.

Product name: PVA Tepla Gigabatch 380M
Year of purchase: 2024

The Plasma Asher 4 can be used for the following processes:

  • Photoresist stripping
  • Descumming
  • Surface cleaning
  • Removal of organic passivation layers and masks


Plasma asher 4 has the following material restrictions:

  • No metals allowed
  • No metal oxides allowed
  • No III-V materials allowed

The user manual, risk assessment, and contact information can be found in LabManager - requires login

Process information

Typical stripping parameters
Tested with 1.5 µm AZ 5214E on 100 mm silicon substrate.

  • O2: 100 sccm
  • N2: 100 sccm
  • Pressure (DSC): 1.3 mbar
  • Power: 1000 W
  • Time (single wafer): 20-30 minutes
  • Time (full boat): 90 minutes


Process development sections