Revision as of 09:41, 25 June 2026 by Mmat (talk | contribs) (Created page with "==Triton-X soap cleaning== 300x300px|thumb|Soap sonic clean placed in the wash bench in the changing room (gowning). The soap sonic is done in a tank with ultrasonics placed in the cleaning bench in the changing room. The cleaning solution is DI water to which a little diluted Triton X-100 is added. Triton X-100 is a non-ionic detergent which is metal ion-free. This detergent is added to reduce surface tension and thus helps removing particles...")
(diff) ← Older revision | Latest revision (diff) | Newer revision → (diff)

Triton-X soap cleaning

 
Soap sonic clean placed in the wash bench in the changing room (gowning).

The soap sonic is done in a tank with ultrasonics placed in the cleaning bench in the changing room. The cleaning solution is DI water to which a little diluted Triton X-100 is added. Triton X-100 is a non-ionic detergent which is metal ion-free. This detergent is added to reduce surface tension and thus helps removing particles from the samples to be cleaned.

Procedure

The bench in the gowning contains a sink, an ultrasonics bath and a rinse bath for rinsing samples cleaned in Triton X-100. To clean the samples:

  • Find a suitable holder for your samples in the cupboard below the baths
  • Make sure the ultrasonics bath dump valve is closed
  • Fill the ultrasonics bath (the one made of metal) with DI water until your samples are completely covered
  • Add 20 - 30 drops of diluted Triton X-100 detergent from the rinse/spray bottle. Do NOT use undiluted Triton X-100
  • Close the bath lid to minimize noise from the ultrasonics bath
  • Start the ultrasound on the front panel
  • Leave the samples in ultrasonics for 10 min
  • Switch off ultrasound
  • Fill the rinse bath (the one made in plastic) with DI water and rinse your samples thoroughly
  • Remove and dry your samples
  • Dump the Triton X-100 solution and rinse bath. Rinse both tanks with DI water. Leave dump valves open so the baths drain completely
  • Continue with Piranha cleaning.