Specific Process Knowledge/Thermal Process/Furnace: Multipurpose annealing/Acceptance test
Feedback to this page: click here
This page is written by DTU Nanolab internal
Multipurpose Anneal furnace acceptance test
The acceptance for the Multipurpose Anneal furnace was performed in November 2014 by ATV Technologie and DTU Nanolab.
At the acceptance test a dry oxide layer was grown on a boat of 150 mm wafers. The oxide growth was repeated three times
For each run the oxide thickness and refractive index were measured on three of the wafers, and the standard deviation and non-uniformity were calculated for each wafer, over the boat and from run to run. The results can be found below.
In November 2024 the furnace was repaired by ATV Technologie. At the repair, the whole furnace body was changed, and all heaters were replaced. Also, the process exhaust flow was decreased by changing a valve in the exhaust line.
After the repair, the acceptance test oxidation process was repeated and optimized. The positions of the control thermocouples (TCs) and the process were adjusted to minimize the the non-uniformity. The final optimized result can be found below.
Oxidation parameters
Recipe: "vr_dryOx_1000C_120min_150_5Wafer_D1_mit_Inliner_oPurgering.ATV"
Oxidation time: 80 min
Temperature: 1050 oC (all temperature zones)
O2 flow: 1 slm
The oxidation has been done with 150 mm wafers. The number of wafers in the boat was 30.
Wafer 4 (towards the door), wafer 16 and wafer 28 (towards the service area) were measured in 13 points using the M-2000V ellipsometer.
Results - Acceptance test 2014
Oxide thickness
| Date | Wafer 4 | Wafer 16 | Wafer 28 | Center point only | |||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | Average oxide thickness [nm] | St. deviation | Non-uniformity [%] | ||
| Run 1 | 28-01-2015 | 109.7 | 1.0 | 1.7 | 107.7 | 0.9 | 1.1 | 106.5 | 0.8 | 1.2 | 107.0 | 2.1 | 1.9 |
| Run 2 | 28-01-2015 | 107.3 | 1.7 | 2.4 | 105.0 | 1.4 | 1.7 | 107.3 | 0.7 | 0.9 | 105.7 | 1.0 | 0.9 |
| Run 3 | 30-01-2015 | 103.6 | 0.8 | 1.1 | 102.6 | 0.6 | 1.2 | 102.2 | 0.6 | 1.1 | 102.9 | 1.0 | 1.0 |
| Average | 106.9 | 1.2 | 1.7 | 105.1 | 1.0 | 1.3 | 105.3 | 0.7 | 1.1 | 105.2 | 1.4 | 1.3 | |
| Run-to-run | ||
|---|---|---|
| Average oxide thickness [nm] | St. deviation | Non-uniformity [%] |
| 105.2 | 2.1 | 2.0 |
Refractive index
| Date | Wafer 4 | Wafer 16 | Wafer 28 | Center point only | |||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Average refractive index | St. deviation | Non-uniformity [%] | Average refractive index | St. deviation | Non-uniformity [%] | Average refractive index | St. deviation | Non-uniformity [%] | Average refractive index | St. deviation | Non-uniformity [%] | ||
| Run 1 | 28-01-2015 | 1.46 | 0.00 | 0.04 | 1.46 | 0.00 | 0.07 | 1.46 | 0.00 | 0.06 | 1.4609 | 0.0004 | 0.0230 |
| Run 2 | 28-01-2015 | 1.46 | 0.00 | 0.09 | 1.46 | 0.00 | 0.17 | 1.44 | 0.01 | 0.69 | 1.4561 | 0.0094 | 05873 |
| Run 3 | 30-01-2015 | 1.46 | 0.00 | 0.06 | 1.46 | 0.00 | 0.05 | 1.46 | 0.00 | 0.07 | 1.4602 | 0.0004 | 0.0291 |
| Average | 1.46 | 0.00 | 0.06 | 1.46 | 0.00 | 0.10 | 1.46 | 0.00 | 0.27 | 1.46 | 0.00 | 0.21 | |
| Run-to-run | ||
|---|---|---|
| Average refractive index | St. deviation | Non-uniformity [%] |
| 1.4591 | 0.0026 | 0.1637 |
Results - Furnace repair 2024
Oxide thickness
| Date | Wafer 4 | Wafer 16 | Wafer 28 | Over the boat (all points) | Center point only | ||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Average oxide thickness [nm] | Non-uniformity [%] | Average oxide thickness [nm] | Non-uniformity [%] | Average oxide thickness [nm] | Non-uniformity [%] | Average oxide thickness [nm] | Non-uniformity [%] | Average oxide thickness [nm] | Non-uniformity [%] | ||
| Test | 07-05-2024 | 108.1 | 0.96 | 108.7 | 0.95 | 109.8 | 0.98 | 108.9 | 0.76 | 108.2 | 1.22 |
Thermo couple (TC) position - Distance from the bell jar: 12 cm, 21.5 cm, 36 m