Etch rate in BHF 1% HF 5% HF 30% HF 40% HF BHF with wetting agent
Wet Thermal Oxide [nm/min] 78.191 / 794 6 24.891 / 32 282.851 794
Pyrex [nm/min] 35 3000
TEOS [nm/min] 265 153
PECVD3 (LFSiO) Oxide [nm/min] 2253
PECVD3 (MFSiNLS2) Nitride [nm/min] 595
PECVD4 (Waveguide) Oxide [nm/min] 1300-14006 1055 / 1086
PECVD4 (HF SiO2) Oxide [nm/min] 2305 / 248±256
Silicon Rich Nitride [nm/min] 0.331 0.601 2.61
Stochiometric Nitride Si3N4 [nm/min] 0.752