Silicon nitride can be etched using either wet chemistry or dry etch equipment. Wet chemistry is mainly used to remove all the nitride on the surface (backside and frontside) of a wafer. Dry etching etches one side at a time and can be used to etch structures with several masking materials.
Comparison of wet Silicon Nitride etch and RIE etch for etching of Silicon Nitride
|
|
Wet Silicon Nitride etch
|
Buffered HF (BHF)
|
RIE
|
| General description
|
- Isotropic etch
- Well suited for removing all nitride on a wafer surface (nitride strip) without a mask. High selectivity Si3N4/Si (>100) and Si3N4/SiO2 (>20) @ 180 C.
|
- Isotropic etch
- Well suited for removing all PECVD nitride on a wafer surface (nitride strip) without a mask. Etches LPCVD nitride very slowly
|
- Anisotropic etch: vertical sidewalls
|
| Possible masking materials
|
- Silicon Oxide
- PolySilicon
|
- Photoresist
- PolySilicon
- Blue film
|
- Photoresist
- Silicon Oxide
- Aluminium
- Chromium (ONLY RIE2!)
- Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)
|
| Etch rate
|
- Si3N4 @ 180 oC: ~84 Å/min
- Si3N4 @ 160 oC: ~60 Å/min
|
- PECVD nitride: ~400-1000 Å/min
|
- Typically 40-50 nm/min can be increased or decreased by using other recipe parameters.
|
| Batch size
|
|
|
|
| Size of substrate
|
|
|
- 4" wafers or smaller pieces
|
| Allowed materials
|
- Silicon
- Silicon Oxide
- Silicon Nitride
- Silicon Oxynitride
|
- Silicon
- Silicon Oxide
- Silicon Nitride
- Silicon Oxynitride
- Photoresist
- Blue film
|
- Silicon
- Silicon Oxide
- Silicon Nitride
- Silicon Oxynitride
- Photoresist
- E-beam resist
- Aluminium
- Chromium (ONLY RIE2!)
- Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)
|